Air Bubble in large panel when slumping.
Moderators: Brad Walker, Tony Smith
-
- Posts: 11
- Joined: Tue May 06, 2008 9:29 pm
Air Bubble in large panel when slumping.
Hi, when slumping a large panel 8" x 15" on a wave mould I always get a large air bubble in the middle of the piece. I have air holes in the mould. The only thing I can think that is causing it is that panel is slight thickness differences in the panel.
-
- Posts: 186
- Joined: Tue Dec 29, 2009 7:13 pm
- Location: Nahant Massachusetts
- Contact:
Re: Air Bubble in large panel when slumping.
Is your mould raised up off of your kiln shelf, if not that could be the problem.
Bob
Bob
-
- Posts: 11
- Joined: Tue May 06, 2008 9:29 pm
Re: Air Bubble in large panel when slumping.
Yes, I have raised it off the kiln floor to let the air escape through the air holes.
-
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
Re: Air Bubble in large panel when slumping.
You could try fiber paper on the mold, or lowering your slump temp. The first solution allows air to escape through the porous paper. The second keeps the glass too stiff for the bubble to be able to expand the glass. I am assuming the bubble is coming from under the glass.
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Re: Air Bubble in large panel when slumping.
What is your schedule and how thick is the piece?
-
- Posts: 11
- Joined: Tue May 06, 2008 9:29 pm
Re: Air Bubble in large panel when slumping.
Hi, the firing schedual is in cent, 85,538,20,85,633,5,465,716,12,Full,488,60,20,445,10,215,150
-
- Posts: 11
- Joined: Tue May 06, 2008 9:29 pm
Re: Air Bubble in large panel when slumping.
Oh yes, the thickness is 3mm with fused frit on top.
-
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
Re: Air Bubble in large panel when slumping.
Do not fire at full speed up to your top temp. 3mm glass picks up heat very quickly. Your fast firing up to top temp is making the glass get too hot and soft. Working with glass thinner than 6mm requires quite a bit of sensitivity.Richard Carder wrote:Oh yes, the thickness is 3mm with fused frit on top.
I'd think about trying 85 633, 170 716 5 Your soaks are a waste of time unless you know something I don't, like glass broke without them. The 5 minute soak can be shortened or extended, as required, to get the job done. If that schedule results in a bubble, either slow down or lower temperature.
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
-
- Posts: 13
- Joined: Tue Mar 13, 2012 12:57 pm
Re: Air Bubble in large panel when slumping.
I had been getting a pesty and persistent air bubble on one piece and I slowed my slump right down and it finally came out brilliant!
-
- Posts: 11
- Joined: Tue May 06, 2008 9:29 pm
Re: Air Bubble in large panel when slumping.
Thanks everyone.
-
- Posts: 321
- Joined: Sat Dec 17, 2005 10:32 pm
- Location: SANTA CRUZ, CALIFORNIA
- Contact:
Re: Air Bubble in large panel when slumping.
Recently i have changed my standard slumping schedule to
300 / 1100. No hold (Slower for thick or tack fused etc)
50 / 1250 then to anneal
Everything has been coming out more evenly slumped and perfect.
I think it all about slowing down at the top.
300 / 1100. No hold (Slower for thick or tack fused etc)
50 / 1250 then to anneal
Everything has been coming out more evenly slumped and perfect.
I think it all about slowing down at the top.
Laurie Spray
New website!! Http://bonnydoonfusedglasstools.com
Maker of stainless steel rings,pattern bar formers, pot melt pots, and Bottomless Molds
glass: http://lauriespray.blogspot.com
New website!! Http://bonnydoonfusedglasstools.com
Maker of stainless steel rings,pattern bar formers, pot melt pots, and Bottomless Molds
glass: http://lauriespray.blogspot.com
-
- Posts: 730
- Joined: Mon Mar 10, 2003 2:22 pm
- Location: wanchese north carolina
- Contact:
Re: Air Bubble in large panel when slumping.
and is the bubble a 'bubble' or a lump resulting from the glass being so soft that is sliding/stretching down into the mold? r.
artist, owner of wanchese art studio, marine finisher
-
- Posts: 11
- Joined: Tue May 06, 2008 9:29 pm
Re: Air Bubble in large panel when slumping.
Just open kiln and my panel is perfect. Thanks everyone for advice.