Crystal irid
Moderators: Brad Walker, Tony Smith
-
PDXBarbara
- Posts: 292
- Joined: Sun Mar 09, 2003 4:09 pm
- Location: Portland, OR
Crystal irid
Got some crystalization on irid. Slumping on kilnwashed (BE wash) SS plate. BE 1116 (turquoise blue) irid down tried to scrub it off (scotchbrite kinda thing, gently w/ wire brush. Actually took off some of the irid. Never seen this before. Usually the irid down helps with the release. Plus the crystalization is specific to one innocuous portion. Ideas on what caused this?
PDXBarbara
PDXBarbara
Barbara Bader
Barbara, does the location and shape of the problem area have any relation to the size and shape of anything slumped on this mold in the past? Different glasses seem to affect kilnwash differently. Some seem to leave more flux in the kilnwash than others as seen by the discoloration of the kilnwash. I know this is more often a problem at fuse temps than slump temps but it is still a possibility here.
Best wishes,
Tom in Texas
Best wishes,
Tom in Texas
-
PDXBarbara
- Posts: 292
- Joined: Sun Mar 09, 2003 4:09 pm
- Location: Portland, OR
Hi Tom. First time slumped on this side of the SS mold. I've used the "normal" side before with fine results. The flip side has a more extreme shape. It was freshly washed (BE wash). Because of the strange shape, I got worried about the SS squeezing the glass upon cooling... so at about 650 F. I shoved the glass askew on the mold so it couldn't catch up in a crevices (about 1/4 inch deep, or so). That was successful.Tom White wrote:Barbara, does the location and shape of the problem area have any relation to the size and shape of anything slumped on this mold in the past? Different glasses seem to affect kilnwash differently. Some seem to leave more flux in the kilnwash than others as seen by the discoloration of the kilnwash. I know this is more often a problem at fuse temps than slump temps but it is still a possibility here.
Best wishes,
Tom in Texas
Oh yeah... while supervise the slump, I added both time & temp. I'd programmed in a burst of heat to get it up to 1300 for a quick polish on some bits I'd sanded & ground. added on about 20 degrees... and kept checking it every 3 -5 minutes...(which kept it from reading too hot, but also kept the elements on than if I'd kept the dang lid shut.) So it hovered around 1300 for about mmmm 15 minutes. polished well... but this irid-on-the-bottom screwup was unexpected.
I'll try plopping the problem area on the scanner ... if it works, you'll see what I mean. Here's a couple pix of pieces molded on the "normal" side. (The crevices are the bottom side of the raised part.)


Last edited by PDXBarbara on Mon Aug 11, 2003 12:07 pm, edited 1 time in total.
Barbara Bader
-
PDXBarbara
- Posts: 292
- Joined: Sun Mar 09, 2003 4:09 pm
- Location: Portland, OR
Here are 2 scans. There are more at http://www.pbase.com/pdxbarbara/crystal ... ystery_pix if ya'll get excited about this problem...PDXBarbara (Bader) wrote:
I'll try plopping the problem area on the scanner ... if it works, you'll see what I mean.
Thanks guys...
BB
In the 2nd pic, the irid scratched off when I tried scrubbing off the white crystals... scrubbed with a scrotchbrite type thing & also tried a stiff brush. I stopped as soon as I saw what was happening.


Barbara Bader
-
Bob
- Posts: 215
- Joined: Mon Mar 10, 2003 1:01 pm
- Location: Salt Spring Island, British Columbia
- Contact:
Hi Barbara,
I am guessing but I have had several irid coatings give the effect in the image. Is the irid surface pitted? Do granules of glass pop out? I have had that occur under two circumstances. One is rare and occurs on fairly "normal" pieces (i.e. I didn't expect a problem). I think your piece falls in this category. I blamed it on being a problem with the glass... perhaps the coating wasn't fully bonded to the glass. From my experience it is pretty rare. The other circumstance is when irid coatings are stretched quite a bit during slumping, particularly over an abrupt edge such as the inside lip of a drop through mold. The problem area on your piece seems to be in the part that would have been slumped most during slumping.... perhaps it was just enough to accent the problem in the glass.
Please don't take this as an informed answer... just some observations.
Cheers,
Bob
I am guessing but I have had several irid coatings give the effect in the image. Is the irid surface pitted? Do granules of glass pop out? I have had that occur under two circumstances. One is rare and occurs on fairly "normal" pieces (i.e. I didn't expect a problem). I think your piece falls in this category. I blamed it on being a problem with the glass... perhaps the coating wasn't fully bonded to the glass. From my experience it is pretty rare. The other circumstance is when irid coatings are stretched quite a bit during slumping, particularly over an abrupt edge such as the inside lip of a drop through mold. The problem area on your piece seems to be in the part that would have been slumped most during slumping.... perhaps it was just enough to accent the problem in the glass.
Please don't take this as an informed answer... just some observations.
Cheers,
Bob
-
PDXBarbara
- Posts: 292
- Joined: Sun Mar 09, 2003 4:09 pm
- Location: Portland, OR
Hi Bob... thanks for helping me out.Bob wrote:Hi Barbara,
I am guessing but I have had several irid coatings give the effect in the image. Is the irid surface pitted? Do granules of glass pop out? I have had that occur under two circumstances. One is rare and occurs on fairly "normal" pieces (i.e. I didn't expect a problem). I think your piece falls in this category. I blamed it on being a problem with the glass... perhaps the coating wasn't fully bonded to the glass. From my experience it is pretty rare. The other circumstance is when irid coatings are stretched quite a bit during slumping, particularly over an abrupt edge such as the inside lip of a drop through mold. The problem area on your piece seems to be in the part that would have been slumped most during slumping.... perhaps it was just enough to accent the problem in the glass.
Please don't take this as an informed answer... just some observations.
Cheers,
Bob
I infer from your description (stretched irid) that as the irid stretches in the extreme part of the slump, it reveals the glass under it. In turn, that leaves the revealed bits vulnerable to devit/crystalizing. (yes?)
However, the swath of crud is actually in the least-slumped part...though adjacent to the most-slumped. Imagine the backside of the piece below. I used the same SS mold, but used the reverse side. So, in the screwed up piece, the irid is on the bottom...against the reverse side of the mold. Thus, the irid (bottom) of the screwed piece is shaped like the one in the pic below.

Here's a better pic of the location of the swath o' crystal weirdness.

So I guess this would fall under your observation #1? Even though the irid was fine during the 2 fuses that preceded the slump?
Thanks again, Bob...
Barbara
Barbara Bader
-
PDXBarbara
- Posts: 292
- Joined: Sun Mar 09, 2003 4:09 pm
- Location: Portland, OR
PS
P.S. your other questions, Bob....
Is the irid surface pitted?
YES.
Do granules of glass pop out?
No. Some of the crystals seem raised, tho.
Muchos gracias again, Bob.
xxoo
BB
Is the irid surface pitted?
YES.
Do granules of glass pop out?
No. Some of the crystals seem raised, tho.
Muchos gracias again, Bob.
xxoo
BB
Barbara Bader
-
Tony Smith
- Posts: 1037
- Joined: Sun Mar 09, 2003 5:59 pm
- Location: Massachusetts, USA
- Contact:
This sounds similar to the irid down problem that I've seen in the past, bust always with a black base glass... you can cratch the irid off with a fingernail and it's pitted under the surface.
no answers... just validation
Tony
no answers... just validation
Tony
The tightrope between being strange and being creative is too narrow to walk without occasionally landing on both sides..." Scott Berkun
-
PDXBarbara
- Posts: 292
- Joined: Sun Mar 09, 2003 4:09 pm
- Location: Portland, OR
Hi Tony...Tony Smith wrote:This sounds similar to the irid down problem that I've seen in the past, bust always with a black base glass... you can cratch the irid off with a fingernail and it's pitted under the surface.
no answers... just validation
Tony
YES. Do you think it's actually devit? Anyway, your description pretty much mirrors my crystal problem, tho mine doesn't involve black.
Have you experienced this problem with System 96 as well as BE?
Do you have any idea what it's from? Maybe I should get in touch w/ Ted Sawyer.
By the way... I've had similar crystalizing on he back of some highfires. But it's during fusing (1700 for 2 hours on fiber)... & irid not involved. (Tho I HAVE seen it on hifires where a sheet of BE irid down on fiber was under the rest of the glass. In that case, the bottom sheet cracked upon AFAP ramp up to process temp, and the crystals definitely congregated along the thermal-shock cracks.)
xxoo,, BB
Barbara Bader
-
Tony Smith
- Posts: 1037
- Joined: Sun Mar 09, 2003 5:59 pm
- Location: Massachusetts, USA
- Contact:
Go back a couple of weeks and read the thread on gold leaf and micas http://www.warmglass.com/phpBB/viewtopic.php?t=1772. I think you'll find that there are a number of people who have experienced this phenomenon with a number of different glasses. Ted Sawyer may be a good person to ask... but don't mention System 96.PDXBarbara (Bader) wrote:Hi Tony...Tony Smith wrote:This sounds similar to the irid down problem that I've seen in the past, bust always with a black base glass... you can cratch the irid off with a fingernail and it's pitted under the surface.
no answers... just validation
Tony
YES. Do you think it's actually devit? Anyway, your description pretty much mirrors my crystal problem, tho mine doesn't involve black.
Have you experienced this problem with System 96 as well as BE?
Do you have any idea what it's from? Maybe I should get in touch w/ Ted Sawyer.
By the way... I've had similar crystalizing on he back of some highfires. But it's during fusing (1700 for 2 hours on fiber)... & irid not involved. (Tho I HAVE seen it on hifires where a sheet of BE irid down on fiber was under the rest of the glass. In that case, the bottom sheet cracked upon AFAP ramp up to process temp, and the crystals definitely congregated along the thermal-shock cracks.)
xxoo,, BB
Tony
The tightrope between being strange and being creative is too narrow to walk without occasionally landing on both sides..." Scott Berkun
-
PDXBarbara
- Posts: 292
- Joined: Sun Mar 09, 2003 4:09 pm
- Location: Portland, OR
I'll look it up, Tony. Thanks for the ref. FYI... Since I used BE glass, System 96 isn't germaine. I only asked you about it cause I have insatiable curiousity. (Like Curious George...)Tony Smith wrote: Go back a couple of weeks and read the thread on gold leaf and micas http://www.warmglass.com/phpBB/viewtopic.php?t=1772. I think you'll find that there are a number of people who have experienced this phenomenon with a number of different glasses. Ted Sawyer may be a good person to ask... but don't mention System 96.
BB
Barbara Bader
it's happened to me on the gold parts of purple translucent irid down against the shelf/mold, against b.e. wash.PDXBarbara (Bader) wrote:I'll look it up, Tony. Thanks for the ref. FYI... Since I used BE glass, System 96 isn't germaine. I only asked you about it cause I have insatiable curiousity. (Like Curious George...)Tony Smith wrote: Go back a couple of weeks and read the thread on gold leaf and micas http://www.warmglass.com/phpBB/viewtopic.php?t=1772. I think you'll find that there are a number of people who have experienced this phenomenon with a number of different glasses. Ted Sawyer may be a good person to ask... but don't mention System 96.
BB
-
PDXBarbara
- Posts: 292
- Joined: Sun Mar 09, 2003 4:09 pm
- Location: Portland, OR
-
Lynne Chappell
- Posts: 186
- Joined: Fri Mar 14, 2003 2:05 am
- Location: Surrey B.C. Canada
- Contact:
i think it may have to do with the phase of the moon.PDXBarbara (Bader) wrote:Hi Charlie.... hmmm.charlie wrote: it's happened to me on the gold parts of purple translucent irid down against the shelf/mold, against b.e. wash.
I guess my next quesion is... do you know why it happened?
Thx.
Pdxbarbara
when iasked lani, she said that there was a batch of be wash that interacted badly with gold irid, when in direct contact. the factory sent me a different batch and i haven't had it replicated since. it looks to me like a bubbling between the irid and glass surfaces, and since it's irid down, the bubbles migrated upwards, causing deep pits in the glass. i would imagine if left for a very long time at fusing temps, they would migrate through the glass to the surface.
in my case, the pits were very large, on the order of 1/16"-1/8" or so in diameter.
-
Tony Smith
- Posts: 1037
- Joined: Sun Mar 09, 2003 5:59 pm
- Location: Massachusetts, USA
- Contact:
the bad container has a code of 121899, the good container code is 012803, which i suspect is a date code. the bad lot probably spans a range of dates.charlie wrote:i don't know offhand, and wasn't told. tonight i'll check the two buckets to see if there's any identifying numbers on them.Tony Smith wrote:Charlie,
Was there a lot number or date associated with this "bad batch" of BE kilnwash???
Tony
-
PDXBarbara
- Posts: 292
- Joined: Sun Mar 09, 2003 4:09 pm
- Location: Portland, OR