Hi Wise-Ones,
I am fusing with system 96 and am using transparent colors- when I slumped into bowl mold, it got 'frosted' on the bottom side.. it was recommended on my next piece I raise the temp (from 1450 to 1470), but that resulted in big bubbles... don't wish to loose more pieces.. any thoughts? If I lower the temp, will that work?
Thanks kindly...
Bonnie
slumping- avoid frosting on backside?
Moderators: Brad Walker, Tony Smith
-
Bonnie Rubinstein
- Posts: 240
- Joined: Sun May 04, 2003 9:04 pm
- Location: River Falls, WI
slumping- avoid frosting on backside?
Bonnie Rubinstein
-
Amy Schleif-Mohr
- Posts: 280
- Joined: Sun Mar 09, 2003 5:18 pm
- Location: Milwaukee
I was having the same problem through experimenting I found although I couldn't eliminate all frosting I reduced it to the upper inch and a half.
results of experiment using spectrum clear - reduce temp. to 1250 or as low as your kiln allows to slump and reduce time to as little as possible.
I reduced time on a 11 3/4" bowl to 5 minutes and still got frostinfg on upper edge, but I like the look so I'm happy.
That is until I want it completely clear.
Val
results of experiment using spectrum clear - reduce temp. to 1250 or as low as your kiln allows to slump and reduce time to as little as possible.
I reduced time on a 11 3/4" bowl to 5 minutes and still got frostinfg on upper edge, but I like the look so I'm happy.
Val
-
Bonnie Rubinstein
- Posts: 240
- Joined: Sun May 04, 2003 9:04 pm
- Location: River Falls, WI
-
Tony Smith
- Posts: 1037
- Joined: Sun Mar 09, 2003 5:59 pm
- Location: Massachusetts, USA
- Contact: