Thanks
slumping overhang
Moderators: Brad Walker, Tony Smith
slumping overhang
I am getting ready to slump and oval platter 12" across by 9". Right now it is 3 layers thick about .300 and I have a 1/4" overhang. I have never slump with an overhang do you think this is too much of an overhang and that I should cold work it and get it down closer.
Thanks
Thanks
-
Bert Weiss
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
One rule of thumb is that an overhang that is the same dimension as the thickness of the glass is OK. You can stretch it a bit more with pretty good luck.
I always try to get the job done with lower temp and more time, until impatience sets in and I bump up the temp to get it over with...
I always try to get the job done with lower temp and more time, until impatience sets in and I bump up the temp to get it over with...
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions