Ceraboard and Hardener

This is the main board for discussing general techniques, tools, and processes for fusing, slumping, and related kiln-forming activities.

Moderators: Brad Walker, Tony Smith

Post Reply
daj
Posts: 2
Joined: Tue Dec 23, 2003 4:47 am
Location: U. K.

Ceraboard and Hardener

Post by daj »

Hi, I would like to make my first attempts at murrine blocks over the Christmas period, using Ceraboard dams to contain the glass.

I can't find any technical info about ceraboard or hardener in my fusing books or on the web, and would be grateful if someone could answer the following.

(1) does ceraboard need pre-firing to remove binder, if so, is 700F for a couple of hours OK?

(2) if treating ceraboard with hardener, what is the sequence of steps? (pre-fire, treat, dry, use) or (pre-fire, treat, dry, re-pre-fire, use) or (treat, dry, pre-fire, use)

Thanks in advance, and happy and safe glassing

David
Peg
Posts: 74
Joined: Tue Apr 08, 2003 7:50 am
Location: Bristol, UK

Post by Peg »

Daj - I don't know what the right way is - but I treat, dry in the kiln, fire out the binder, use.
It can get a bit soggy and friable when wet, so maybe air-drying would be a good move.

Oh, and it stinks when prefiring out the binder.

Where are you in the UK?
Bert Weiss
Posts: 2339
Joined: Tue Mar 11, 2003 12:06 am
Location: Chatham NH
Contact:

Re: Ceraboard and Hardener

Post by Bert Weiss »

daj wrote:Hi, I would like to make my first attempts at murrine blocks over the Christmas period, using Ceraboard dams to contain the glass.

I can't find any technical info about ceraboard or hardener in my fusing books or on the web, and would be grateful if someone could answer the following.

(1) does ceraboard need pre-firing to remove binder, if so, is 700F for a couple of hours OK?

(2) if treating ceraboard with hardener, what is the sequence of steps? (pre-fire, treat, dry, use) or (pre-fire, treat, dry, re-pre-fire, use) or (treat, dry, pre-fire, use)

Thanks in advance, and happy and safe glassing

David
David

I don't think that 700ºF is hot enough. I would fire it to the temp you plan to use it at. Once it turns back to white from black it is good. The job will get done faster at the hotter temps.

I have never rigidized so I can't help you there.
Bert

Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Brad Walker
Site Admin
Posts: 1542
Joined: Fri Mar 07, 2003 9:33 pm
Location: North Carolina, USA
Contact:

Post by Brad Walker »

I would prefire to 1400F and soak for just a few minutes. You'll know the binder is out if the color turns back to white. 700F is definitely too low, and a couple of hours is too long.

I believe that Ceraboard is a rigid product (right?), and will stand on edge. If so, then you shouldn't need to rigidize it to use as a dam material. Just cut and line with fiber paper or kiln wash well.
Brad Walker
Site Admin
Posts: 1542
Joined: Fri Mar 07, 2003 9:33 pm
Location: North Carolina, USA
Contact:

Post by Brad Walker »

Brad Walker wrote:I would prefire to 1400F and soak for just a few minutes. Leave the kiln open about an inch until the temperature gets above 1000F. It will stink and may smoke a little. You'll know the binder is out if the color turns back to white. 700F is definitely too low, and a couple of hours is too long.

I believe that Ceraboard is a rigid product (right?), and will stand on edge. If so, then you shouldn't need to rigidize it to use as a dam material. Just cut and line with fiber paper or kiln wash well.
Tony Serviente
Posts: 328
Joined: Thu May 29, 2003 11:48 am
Location: Ithaca,NY
Contact:

Post by Tony Serviente »

I've used rigidizer with ceramic fiber batt, and did not pre fire before applying rigidizer. It worked well. I would actually caution against firing first and then applying, as the fiber will be much more friable and will present a greater handling(and safety) problem.
Cheryl
Posts: 239
Joined: Sun Mar 09, 2003 7:56 pm
Location: Tallahassee FL
Contact:

so to use ceramaboard as a kiln shelf...

Post by Cheryl »

which I will only do when I need the full length of my bathtub kiln, I know that drill...

I should cut to fit the kiln, then rigidize, let dry, then fire sans glass? Does it need multiple coats of rigidizer?
Brock
Posts: 1519
Joined: Mon Mar 10, 2003 1:32 pm
Location: Vancouver, B.C.

Re: so to use ceramaboard as a kiln shelf...

Post by Brock »

Cheryl wrote:which I will only do when I need the full length of my bathtub kiln, I know that drill...

I should cut to fit the kiln, then rigidize, let dry, then fire sans glass? Does it need multiple coats of rigidizer?
It shouldn't, but you must saturate it.

Cut to shape/size, soak in rigidizer, air dry, (or force with heat if you like)
pre-fire, finish (smooth/sand), kiln wash, fire, then . . . use. Brock
Cheryl
Posts: 239
Joined: Sun Mar 09, 2003 7:56 pm
Location: Tallahassee FL
Contact:

whew!

Post by Cheryl »

Thanks, Brock.

PS: How're you feeling after el accidente?
daj
Posts: 2
Joined: Tue Dec 23, 2003 4:47 am
Location: U. K.

Post by daj »

Thank you to everyone who has taken the time and trouble to reply to my question - espec to Brock for his caution about needing to apply kiln wash, I had assumed that I wouldn't need to do it. Now I just need to find the time to fire up the kiln.

David
Post Reply