Hi, I would like to make my first attempts at murrine blocks over the Christmas period, using Ceraboard dams to contain the glass.
I can't find any technical info about ceraboard or hardener in my fusing books or on the web, and would be grateful if someone could answer the following.
(1) does ceraboard need pre-firing to remove binder, if so, is 700F for a couple of hours OK?
(2) if treating ceraboard with hardener, what is the sequence of steps? (pre-fire, treat, dry, use) or (pre-fire, treat, dry, re-pre-fire, use) or (treat, dry, pre-fire, use)
Thanks in advance, and happy and safe glassing
David
I can't find any technical info about ceraboard or hardener in my fusing books or on the web, and would be grateful if someone could answer the following.
(1) does ceraboard need pre-firing to remove binder, if so, is 700F for a couple of hours OK?
(2) if treating ceraboard with hardener, what is the sequence of steps? (pre-fire, treat, dry, use) or (pre-fire, treat, dry, re-pre-fire, use) or (treat, dry, pre-fire, use)
Thanks in advance, and happy and safe glassing
David
-
Bert Weiss
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
Re: Ceraboard and Hardener
Daviddaj wrote:Hi, I would like to make my first attempts at murrine blocks over the Christmas period, using Ceraboard dams to contain the glass.
I can't find any technical info about ceraboard or hardener in my fusing books or on the web, and would be grateful if someone could answer the following.
(1) does ceraboard need pre-firing to remove binder, if so, is 700F for a couple of hours OK?
(2) if treating ceraboard with hardener, what is the sequence of steps? (pre-fire, treat, dry, use) or (pre-fire, treat, dry, re-pre-fire, use) or (treat, dry, pre-fire, use)
Thanks in advance, and happy and safe glassing
David
I don't think that 700ºF is hot enough. I would fire it to the temp you plan to use it at. Once it turns back to white from black it is good. The job will get done faster at the hotter temps.
I have never rigidized so I can't help you there.
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
-
Brad Walker
- Site Admin
- Posts: 1542
- Joined: Fri Mar 07, 2003 9:33 pm
- Location: North Carolina, USA
- Contact:
I would prefire to 1400F and soak for just a few minutes. You'll know the binder is out if the color turns back to white. 700F is definitely too low, and a couple of hours is too long.
I believe that Ceraboard is a rigid product (right?), and will stand on edge. If so, then you shouldn't need to rigidize it to use as a dam material. Just cut and line with fiber paper or kiln wash well.
I believe that Ceraboard is a rigid product (right?), and will stand on edge. If so, then you shouldn't need to rigidize it to use as a dam material. Just cut and line with fiber paper or kiln wash well.
-
Brad Walker
- Site Admin
- Posts: 1542
- Joined: Fri Mar 07, 2003 9:33 pm
- Location: North Carolina, USA
- Contact:
Brad Walker wrote:I would prefire to 1400F and soak for just a few minutes. Leave the kiln open about an inch until the temperature gets above 1000F. It will stink and may smoke a little. You'll know the binder is out if the color turns back to white. 700F is definitely too low, and a couple of hours is too long.
I believe that Ceraboard is a rigid product (right?), and will stand on edge. If so, then you shouldn't need to rigidize it to use as a dam material. Just cut and line with fiber paper or kiln wash well.
-
Tony Serviente
- Posts: 328
- Joined: Thu May 29, 2003 11:48 am
- Location: Ithaca,NY
- Contact:
so to use ceramaboard as a kiln shelf...
which I will only do when I need the full length of my bathtub kiln, I know that drill...
I should cut to fit the kiln, then rigidize, let dry, then fire sans glass? Does it need multiple coats of rigidizer?
I should cut to fit the kiln, then rigidize, let dry, then fire sans glass? Does it need multiple coats of rigidizer?
Re: so to use ceramaboard as a kiln shelf...
It shouldn't, but you must saturate it.Cheryl wrote:which I will only do when I need the full length of my bathtub kiln, I know that drill...
I should cut to fit the kiln, then rigidize, let dry, then fire sans glass? Does it need multiple coats of rigidizer?
Cut to shape/size, soak in rigidizer, air dry, (or force with heat if you like)
pre-fire, finish (smooth/sand), kiln wash, fire, then . . . use. Brock