I tried to drape a piece of fused BE glass over a crest mold coated with glass serarator.  The glass has stuck to the mold.  Does anybody have ANY ideas on how I can get the glass off the mold?.  Thanks for your help.
Bob
			
			
									
						
										
						Help! I'm stuck
Moderators: Brad Walker, Tony Smith
- 
				Kim Bellis
- Posts: 133
- Joined: Sat Jun 14, 2003 9:48 pm
- Location: Tampa, Florida
- Contact:
- 
				Judy Schnabel
- Posts: 195
- Joined: Mon Mar 10, 2003 9:45 pm
- Location: SW FL
- Contact:
- 
				Robert Cohen
Help! I'm stuck.
Kim, Judy & YoDuh.  Thanks for your input.  I finally called Crest Molds who suggested that I soak the mold for awhile and then tap gently with a rubber mallet.  I did just that and guess what?  I broke the glass  However I did save the mold which I guess is a plus.  From now on, despite what Crest Mold advertises, I'm going to use thinfire paper with their molds and follow Judys advice.  Thanks again for your help.
  However I did save the mold which I guess is a plus.  From now on, despite what Crest Mold advertises, I'm going to use thinfire paper with their molds and follow Judys advice.  Thanks again for your help.
Bob
			
			
									
						
										
						 However I did save the mold which I guess is a plus.  From now on, despite what Crest Mold advertises, I'm going to use thinfire paper with their molds and follow Judys advice.  Thanks again for your help.
  However I did save the mold which I guess is a plus.  From now on, despite what Crest Mold advertises, I'm going to use thinfire paper with their molds and follow Judys advice.  Thanks again for your help.Bob
- 
				Gale aka artistefem
- Posts: 184
- Joined: Sun Mar 09, 2003 8:14 pm
- Location: MO-on the banks of the Mississippi
- Contact:
There are a couple other solutions....... to save the mold - reheat the mold and glass till the glass has reached a softened state.  Reach in the kiln and pull the glass off the mold.
The way to prevent sticking and save the glass is more preventative. On the cool down when your kiln temp is in the 1100-1125 degree range, shut off the kiln (for just a few seconds), lift the lid.
I reach into my kiln with a three foot piece of metal flat strap that has a hook bent in the end of it. I gently hook the edge of the glass, lifting it up off the mold. I maneuver the glass just enough that it doesn't settle back down into it's original contact points with the mold.
You have to be quick about this so you don't lose too much kiln heat. If your temp drops below 1075, take the temp back up to 1100 degrees and finish out your cool down annealing cycle.
I've done this for years with my problematic (usually large and high)drape molds with no visible (checked with polarizing film) glass stress.
Any of you wise old glass-ies care to comment on whether this is a good practice?
			
			
									
						
										
						The way to prevent sticking and save the glass is more preventative. On the cool down when your kiln temp is in the 1100-1125 degree range, shut off the kiln (for just a few seconds), lift the lid.
I reach into my kiln with a three foot piece of metal flat strap that has a hook bent in the end of it. I gently hook the edge of the glass, lifting it up off the mold. I maneuver the glass just enough that it doesn't settle back down into it's original contact points with the mold.
You have to be quick about this so you don't lose too much kiln heat. If your temp drops below 1075, take the temp back up to 1100 degrees and finish out your cool down annealing cycle.
I've done this for years with my problematic (usually large and high)drape molds with no visible (checked with polarizing film) glass stress.
Any of you wise old glass-ies care to comment on whether this is a good practice?