Tack Fusing on Irid Surface
Moderators: Brad Walker, Tony Smith
Tack Fusing on Irid Surface
Does anyone regularly or semi-regularly tack fuse onto an irid surface? Is there a chance that the tack fused pieces will "pop" off at a later date? Out of a grouping of 2 dozen plates/trays, while slump firing, I had one tack fused piece (dichroic noodle) split then pop off. I realize that the area of a noodle is small indeed so that might be a factor. I've fixed it now and would love any thoughts/solutions.
Thanks in advance.
RobinE
			
			
									
						
										
						Thanks in advance.
RobinE
- 
				Tony Smith
- Posts: 1037
- Joined: Sun Mar 09, 2003 5:59 pm
- Location: Massachusetts, USA
- Contact:
The etching cream will remove some of the irids. I've had luck removing the Spectrum and the Uroboros Irid (although I've had some feedback that the Uro Irid doesn't always etch off). The Bullseye irid is the toughest and etching cream won't even touch it.
Tony
			
			
									
						
							Tony
The tightrope between being strange and being creative is too narrow to walk without occasionally landing on both sides..."   Scott Berkun
			
						- 
				Bob
- Posts: 215
- Joined: Mon Mar 10, 2003 1:01 pm
- Location: Salt Spring Island, British Columbia
- Contact:
Hi Robin,
I have worked with tack fused beads on irid surfaces and had some popping off. Some of it was caused by trying to tack fuse irid on irid.... just didn't work. When only one surface is irid it seemed to work OK if I took the temp to 1345F (hotter than I regularly tack fuse (1325)) and soaked it for 30 minutes. Perhaps the small mass of the beads makes it difficult to bond onto the surface.
Hope this helps.
Cheers,
Bob
			
			
									
						
										
						I have worked with tack fused beads on irid surfaces and had some popping off. Some of it was caused by trying to tack fuse irid on irid.... just didn't work. When only one surface is irid it seemed to work OK if I took the temp to 1345F (hotter than I regularly tack fuse (1325)) and soaked it for 30 minutes. Perhaps the small mass of the beads makes it difficult to bond onto the surface.
Hope this helps.
Cheers,
Bob
- 
				judith
- Posts: 49
- Joined: Tue Mar 11, 2003 8:57 am
- Location: Vitrum Studio - Maryland - DC area
- Contact:
Robin,
Another easy way to get bettter adherence is to use a bit of clear powder between the design element and the irid surface. Just coat the back of the design element with a bit of GlasTac (or something similar) and dip it into clear powder. Then place it, powder side down, on the irid surface and fire. The powder will melt quickly and invisibly and fuse the surfaces together.
judith
			
			
									
						
										
						Another easy way to get bettter adherence is to use a bit of clear powder between the design element and the irid surface. Just coat the back of the design element with a bit of GlasTac (or something similar) and dip it into clear powder. Then place it, powder side down, on the irid surface and fire. The powder will melt quickly and invisibly and fuse the surfaces together.
judith
- 
				Duane Sitton
- Posts: 7
- Joined: Sun May 11, 2003 6:30 am
- Location: Independence, KS
I've been using the clear powder for some time too, it also seems to help fusing dichro frit to dichro.judith wrote:Robin,
Another easy way to get bettter adherence is to use a bit of clear powder between the design element and the irid surface. Just coat the back of the design element with a bit of GlasTac (or something similar) and dip it into clear powder. Then place it, powder side down, on the irid surface and fire. The powder will melt quickly and invisibly and fuse the surfaces together.
judith
An added benifit of the clear powder on the jewelery pieces I do is it helps keeps small elements in place. Kinda like putting sand under a car tire on ice, it gives it some "traction".
Regards,
Duane
- 
				Tony Serviente
- Posts: 328
- Joined: Thu May 29, 2003 11:48 am
- Location: Ithaca,NY
- Contact:
I've been tack fusing spectrum irid to irid for many years, with no pop offs. I fire to a temp that gives a gently rounded edge to the tacked decorative elements, but still shows the irid well. Too hight and the irid is absorbed, too low and the edges are sharp, and the tack is poor. I have a line based on face up tacks of irid to irid, and if pop offs were a problem, I would have heard about. I have only done this with Spectrum, and do not know if it will work as well with BE.
			
			
									
						
										
						Irid breakdown
OK - I am getting some "pulling/alligator skin" sometimes around my tack fused pieces to irid. This doesn't happen anywhere else - just between tack fused elements that are spaced anywhere from 1/8" to 1/2" apart from eachother. And it isn't consistent with a color. I am doing this series in 6 diff colors.
Here's what I think:
- the tack fuse temp is too high or high/long
- I'm stacking and this tends to happen less on the glass that is on a lower shelf (my kiln is 13" deep)
- I will next try Judith's suggestion of glass tac/clear powder or fine under elements to be tack fused
Thoughts?
Thank you
Robin E
			
			
									
						
										
						Here's what I think:
- the tack fuse temp is too high or high/long
- I'm stacking and this tends to happen less on the glass that is on a lower shelf (my kiln is 13" deep)
- I will next try Judith's suggestion of glass tac/clear powder or fine under elements to be tack fused
Thoughts?
Thank you
Robin E
- 
				Bob
- Posts: 215
- Joined: Mon Mar 10, 2003 1:01 pm
- Location: Salt Spring Island, British Columbia
- Contact:
Hi Robin,
What is the thickness of the base glass that you are tack fusing onto? If it is 1/8" then the glass may be contracting due to surface tension. The irid coating puckers as the glass contracts. If the base glass is 1/4" thick then it should not change volume ... in theory. I have never had what you describe for bases that were 1/4" thick.
The only other possibility is that you have a mix of hard and soft glasses and the slight differences in melting temperature is causing puckering... just another guess.
Hope this helps.
Cheers,
Bob
			
			
									
						
										
						What is the thickness of the base glass that you are tack fusing onto? If it is 1/8" then the glass may be contracting due to surface tension. The irid coating puckers as the glass contracts. If the base glass is 1/4" thick then it should not change volume ... in theory. I have never had what you describe for bases that were 1/4" thick.
The only other possibility is that you have a mix of hard and soft glasses and the slight differences in melting temperature is causing puckering... just another guess.
Hope this helps.
Cheers,
Bob
- 
				Debinsandiego
- Posts: 41
- Joined: Mon May 19, 2003 6:47 pm
HI Bob:
Thanks for your thoughts. The blanks that are puckering have already been fired. They are 1/4". And the tack fused elements are a harder glass than the base 1/4" blanks.
I think I solved my problem today. We had moved my kiln from being outside into in the garage a few weeks ago. I readjusted my firing schedule and the todays batch came out great.
This stuff always keeps me on my toes.
Robin
			
			
									
						
										
						Thanks for your thoughts. The blanks that are puckering have already been fired. They are 1/4". And the tack fused elements are a harder glass than the base 1/4" blanks.
I think I solved my problem today. We had moved my kiln from being outside into in the garage a few weeks ago. I readjusted my firing schedule and the todays batch came out great.
This stuff always keeps me on my toes.
Robin