So, okay, I tried it again.  This time I went to 1750, with a 30 minute soak.  I also added more pieces of glass to the pots, since they weren't very full and hadn't really melted anyway.  
The glass all oozed out just the way it was supposed to.  There was lots of sparkle since I had a number of scraps of green aventurine BE sheet glass, along with the iridized.  Didn't see any of the dichro crumbs, but wasn't too surprised. 
It was still at about 275 degrees when I looked at it closely.  Of course I got the dreaded tink, tink, tink.  I assume it was thermal shock.  
](./images/smilies/eusa_wall.gif)
  The other possibility was incompatibility issues with the aventurine.  Everything was BE or Uroboros 90, but I know that doesn't always matter.  Also in the mix was some clear, clear with frit and streamers, the iridized black, some iridized clear,  and a few miscellaneous pieces of blues, pinks, etc.  Like I say, I was playing with scraps.
Of that unholy mix is there anything that doesn't like to play together? 