I am just starting my sefl formation on glass fusion thanks to this site and all your information on the forum. I have done ceramic for quite a while but also havent toutched it for a while. Now my question is: If I make a mold of plaster and chamotte(grog) can it be reusable and how much. If not, would you guys have a better solution for me?
reusing plaster mold
Moderators: Brad Walker, Tony Smith
-
east-coast-jacques
- Posts: 4
- Joined: Fri Feb 13, 2004 10:36 am
- Location: Caraquet, NB, Canada
- Contact:
reusing plaster mold
Hi all,
I am just starting my sefl formation on glass fusion thanks to this site and all your information on the forum. I have done ceramic for quite a while but also havent toutched it for a while. Now my question is: If I make a mold of plaster and chamotte(grog) can it be reusable and how much. If not, would you guys have a better solution for me?

I am just starting my sefl formation on glass fusion thanks to this site and all your information on the forum. I have done ceramic for quite a while but also havent toutched it for a while. Now my question is: If I make a mold of plaster and chamotte(grog) can it be reusable and how much. If not, would you guys have a better solution for me?
There is a fine line between a hobby and loosing your mind...
Jacques
Jacques
-
Ron Coleman
- Posts: 468
- Joined: Sun Mar 09, 2003 3:20 pm
- Location: Columbus, Ohio USA
Heat destroys the chemical composition of plaster and it will start to fall apart during the first firing, even with grog added.
Since you know how to work with clay, try some raku clay and form your molds and then bisque fire them. After bisque firing add some kiln wash and you will have a mold good for many trips to the kiln.
Ron
Since you know how to work with clay, try some raku clay and form your molds and then bisque fire them. After bisque firing add some kiln wash and you will have a mold good for many trips to the kiln.
Ron
clay
Ron advice pls.....Just make my own molds with raku (you inspired me) they have been sitting lightly covered with plastic but dont seem to be drying out? How long should this take. It is cold in my garage....Ill have real mold soon......green
Then when I do fire...can u give me a firing schedule for jen ken 24".........
Re: clay
you need some air circulation and a way to export water.doctac wrote:Ron advice pls.....Just make my own molds with raku (you inspired me) they have been sitting lightly covered with plastic but dont seem to be drying out? How long should this take. It is cold in my garage....Ill have real mold soon......greenThen when I do fire...can u give me a firing schedule for jen ken 24".........
dry them on wallboard, or cover with newspaper and replace daily.
if it's humid out, it could take weeks to dry them.
firing schedule i use is
400 850 0
100 1050 0
400 1650 30
off. cool to room temp without opening.
-
Bert Weiss
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
Re: reusing plaster mold
Jacqueseast-coast-jacques wrote:Hi all,
I am just starting my sefl formation on glass fusion thanks to this site and all your information on the forum. I have done ceramic for quite a while but also havent toutched it for a while. Now my question is: If I make a mold of plaster and chamotte(grog) can it be reusable and how much. If not, would you guys have a better solution for me?
Ron's suggestion is a good one. For a more complete description of mold making techniques for glass get Boyce Lundstrom's book "Glass Casting and Mold Making, book 3" Click on the Whitehouse books sponsor link.
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions