thanks!
exploding glass
Moderator: Tony Smith
exploding glass
Hi- Newbie here. Hoping someone can help me understand why my glass exploded when trying to make a pocket vase.
I used a piece of 1" fiber board as the form for the pocket. Using Bulleye 90 COE. I have a Paragon QuickKiln 6 with a controller. I set the controller @ 1.5 and after 10 min I heard the distinctive sound of glass cracking. Suggestions/ words of wisdom to overcome this boo- boo?
thanks!
thanks!
-
Bert Weiss
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
Re: exploding glass
Fiber board is an insulator. It looks like you heated up to a point where the temperature gradient within one piece of the glass was great enough to cause a thermal shock crack.
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Re: exploding glass
thanks so much for the fast response.
I'll try using fiber paper next time.
-
rosanna gusler
- Posts: 730
- Joined: Mon Mar 10, 2003 2:22 pm
- Location: wanchese north carolina
- Contact:
Re: exploding glass
fiber paper is an insulator too. you have to slow way down on those vases. also annealing needs to be longer. rosanna
artist, owner of wanchese art studio, marine finisher