Thermal Shock Cracking Whilst Slumping
Moderators: Brad Walker, Tony Smith
-
Richard Carder
- Posts: 11
- Joined: Tue May 06, 2008 9:29 pm
Thermal Shock Cracking Whilst Slumping
I have just slumped a dish 11" square. The total thickness of the dish is 6mm, Bullseye glass. The kiln that I am using is a Paragon Fusion 8. The firing schedule whilst annealing is 522c for 1 hour. When I opened the kiln there was a clean crack along the centre of the dish. There must be something wrong with my firing schedule, can anyone help?
-
Bert Weiss
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
Re: Thermal Shock Cracking Whilst Slumping
Most often, this crack will come from heating up too fast. Slow down. There have been a constant stream of people who post, "This schedule has always worked for me before" Sometimes you have to be more conservative during the heatup. Slumps are particularly difficult because the glass contacts the mold in places and is open to the air in others.
I don't know your kiln, but many kilns will anneal 6mm to a point where it won't crack in the kiln, with a simple shut off. I am not saying don't run an anneal schedule for this thickness.
Slump firings can be difficult to determine if the cracked edge is sharp or rounded. If the crack happens during the heatup, the edge will be exposed to the highest heat in the cycle. If it is hot enough for long enough, the edge will round. Fuse firings are easy to tell the difference.
I don't know your kiln, but many kilns will anneal 6mm to a point where it won't crack in the kiln, with a simple shut off. I am not saying don't run an anneal schedule for this thickness.
Slump firings can be difficult to determine if the cracked edge is sharp or rounded. If the crack happens during the heatup, the edge will be exposed to the highest heat in the cycle. If it is hot enough for long enough, the edge will round. Fuse firings are easy to tell the difference.
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
-
Richard Carder
- Posts: 11
- Joined: Tue May 06, 2008 9:29 pm
Re: Thermal Shock Cracking Whilst Slumping
Thanks for your reply. The edge of the glass where it cracked is rounded, so it make me think that it cracked during heating up, so I will slow it down.
Re: Thermal Shock Cracking Whilst Slumping
Slow down is probably good advice, but what *is* your schedule? Your complete schedule, start to finish? And what are you slumping into?
Cynthia Morgan
Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery
http://www.cynthiamorgan.com
"I wrote, therefore I was." (me)
Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery
http://www.cynthiamorgan.com
"I wrote, therefore I was." (me)