Kiln Problem
Moderators: Brad Walker, Tony Smith
-
jim burchett
- Posts: 255
- Joined: Sun Jun 29, 2003 4:24 pm
- Location: Lenoir, NC
Kiln Problem
Hi Y'all. I have a GlassGlow 450 kiln that I love but recently i have been having a problem. I was having bits of rust and flakes of material falling into the firing chamber..I searched and searched and couldnt figure out where they were coming from. At last while closing the kiln I saw some pieces falling out between the SS lid shell and the fiberboard interior. I have since then gone along tapping on the lid to loosen these flakes and try to get them to clear also vacuum the joint multiple times..yet it seems impossible to get it all and flakes continue to fall down and contaminate the work inside. I dont see any easy way to remove the skin to clean it. Has anyone else had a similar problem? Is there a refractory caulk that I can seal the seam with? any help will be appreciated. I have written to Phil and await his suggestions. Thanks
"No, you cant scare Me, I'm sticking to the UNION. I'm stickin to the UNION till the day I die" Woody Guthrie
-
Valerie Adams
- Posts: 587
- Joined: Mon Apr 19, 2004 2:49 pm
- Location: Santa Rosa, California
- Contact:
Re: Kiln Problem
I'd see what Phil has to say first, but I've used Pyrolite high-temperature caulking to repair the drooping elements in my kiln's lid.
Re: Kiln Problem
LDS Moldable Fiberfrax by Unifrax - got some from Ed Hoy's through my retailer.jim burchett wrote:Is there a refractory caulk that I can seal the seam with? Thanks
Jerry
-
Bert Weiss
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
Re: Kiln Problem
Jim
I don't understand why stainless steel would be raining rust?
I don't understand why stainless steel would be raining rust?
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Re: Kiln Problem
The rust is from the frame . . .
-
jim burchett
- Posts: 255
- Joined: Sun Jun 29, 2003 4:24 pm
- Location: Lenoir, NC
Re: Kiln Problem
I dont either but it is..Phil said he had found some caulk that might work and will send it to me. I'm hoping because it is a PITA! Have to cover the opening with cardboard as I close the lid to catch most of it, then slip the Cardboard out as the lid closes and hope nothing else falls.
"No, you cant scare Me, I'm sticking to the UNION. I'm stickin to the UNION till the day I die" Woody Guthrie
Re: Kiln Problem
Whoa. I believe I would stop loving that kiln. And be doing a lot of surface grinding!
Cynthia Morgan
Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery
http://www.cynthiamorgan.com
"I wrote, therefore I was." (me)
Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery
http://www.cynthiamorgan.com
"I wrote, therefore I was." (me)
-
Bert Weiss
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
Re: Kiln Problem
If the frame is made of mild steel, I would consider cutting it apart and replacing the pieces that see the heat with 304 stainless steel. Once at a school, I had to work with a kiln that rained rust and I found it horrid.
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
-
jim burchett
- Posts: 255
- Joined: Sun Jun 29, 2003 4:24 pm
- Location: Lenoir, NC
Re: Kiln Problem
Believe me I am hoping that the "fix from Phil works, otherwise I will have to do something. Nothing is easily accessible, as Bert indicated I'll have to "skin" it, and I dont really want to do that.
"No, you cant scare Me, I'm sticking to the UNION. I'm stickin to the UNION till the day I die" Woody Guthrie
-
Rick Wilton
- Posts: 273
- Joined: Sat Oct 25, 2003 8:18 pm
- Location: Calgary, Canada
- Contact:
Re: Kiln Problem
How big is the space? Can you pack some fibre paper, blanket, board or rope into the space?
Rick Wilton
-
Valerie Adams
- Posts: 587
- Joined: Mon Apr 19, 2004 2:49 pm
- Location: Santa Rosa, California
- Contact:
Re: Kiln Problem
Phil is the builder of these kilns, right? I would expect that he'd have the proper fix for you, without you having to do a lot of rigging.
-
jim burchett
- Posts: 255
- Joined: Sun Jun 29, 2003 4:24 pm
- Location: Lenoir, NC
Re: Kiln Problem
Valerie, that is what I am hoping..it is a paper thin space where the fiber inner lid butts against the SS outer lid, filtering down as the lid is closed spreading throughout the kiln.
"No, you cant scare Me, I'm sticking to the UNION. I'm stickin to the UNION till the day I die" Woody Guthrie