Hello people..
i was away from here from a lot...but here is me again ;)

I would like to ask a tecnical question.

In Italy we use to protect a sandblasted glass with a liquid anti-fingertip.

Since i have to do a tempered sandblasted door, if i sandblast the glass before i "temper" the glass...can i avoid further fingertip without use the liquid?

Can tempering a sandblasted glass get a satin effect against finger-tip ?

i would appreciate your opinion

thanks in advance.

bye

mike from italy
thanks for sharing !

mike from italy


"secret of success?... passion & experience"

http://www.picturetrail.com/mikefromitaly
Stephen Richard
Posts: 302
Joined: Sun Jul 06, 2003 4:36 pm
Location: Glasgow, Scotland
Contact:

Re: sandblasting before or after ?

Post by Stephen Richard »

probably, but you need to do a test
Steve Richard
You can view my Blog at: http://verrier-glass.blogspot.com/
Bert Weiss
Posts: 2339
Joined: Tue Mar 11, 2003 12:06 am
Location: Chatham NH
Contact:

Re: sandblasting before or after ?

Post by Bert Weiss »

Tempering only goes to 600ºC, so I do not think that is hot enough to effect the blasted surface.

The glass will be stronger if you blast first and then temper. If you temper first, then blast, the glass is weakened by changing the surface.

If you happen to be deep carving with the blaster, it can help to first heat to around 600ºC and then anneal the glass before you temper it. I've heard of people having problems with breakage while tempering sand carved glass. If it is just a surface frost, I do not think there will be a problem.
Bert

Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Buttercup
Posts: 638
Joined: Mon Jan 28, 2008 5:22 pm
Location: S.E. Queensland Australia

Re: sandblasting before or after ?

Post by Buttercup »

....and if your supplier accidently sends you tempered glass, without an identifying logo, for carving, be prepared for an explosion like a shotgun blast as the whole thing blows to pieces. Very frustrating when you've already masked and cut the artwork for several pieces. Jen
Don Burt
Posts: 580
Joined: Sun Mar 09, 2003 8:45 pm
Location: Bloomington, Indiana
Contact:

Re: sandblasting before or after ?

Post by Don Burt »

Buttercup wrote:....and if your supplier accidently sends you tempered glass, without an identifying logo, for carving, be prepared for an explosion like a shotgun blast as the whole thing blows to pieces. Very frustrating when you've already masked and cut the artwork for several pieces. Jen
Aw, sorry. Wish I'd seen the video though.
Buttercup
Posts: 638
Joined: Mon Jan 28, 2008 5:22 pm
Location: S.E. Queensland Australia

Re: sandblasting before or after ?

Post by Buttercup »

Fortunately the masking held most of it in one clump....or were you talking about the video of me hitting the roof of the booth? :shock:
Post Reply