ummm ,,,what happened??

This forum is for questions from newcomers to kiln-forming.

Moderator: Tony Smith

Post Reply
Paul Schulz
Posts: 49
Joined: Mon Apr 01, 2013 10:02 pm
Location: Christchurch New Zealand

ummm ,,,what happened??

Post by Paul Schulz »

Hi guys what happened to this ?? using COE96 spectrum and bullseye glass (bullseye Tekta as the base for the stringers)the full fuse program was as follow
480 per hour to 932 hold 20 minutes
asap to 1490 hold 60 mins
asap to 906 hold 60 mins
150 per hour to 200
had no problems with the fusing the blank lay around the studio for a few days
but when i stumped the piece as follows
572 per hour to 932 hold 20 mins
asap to 1202 hold 20 mins
asap to 899 hold 60 mins
212 per hour to 698
626 per hour to 176
the blank is 6 mm thick
i took the plate out at room temp ,,put it on a table top and bang!!! ,,blew up ,,it was quite cool to touch
Attachments
stringer plate 002.jpg
stringer plate 001.jpg
beninfl
Posts: 46
Joined: Sat Feb 08, 2014 8:54 pm

Re: ummm ,,,what happened??

Post by beninfl »

You cant fuse Bullseye Glass (COE 90) and Spectrum Glass (COE 96) into the same piece. They are not compatible. They will do this every time. Use Bullseye only with Bullseye, and Spectrum only with Spectrum.
Marty
Posts: 865
Joined: Mon Mar 10, 2003 3:58 pm
Location: Maine
Contact:

Re: ummm ,,,what happened??

Post by Marty »

and slow your schedules down!
beninfl
Posts: 46
Joined: Sat Feb 08, 2014 8:54 pm

Re: ummm ,,,what happened??

Post by beninfl »

Yea, that schedule is extremely weird. Such precise numbers, for what reason? 572 per hour? 626 per hour? 212 per hour to 698?
Tony Smith
Posts: 1037
Joined: Sun Mar 09, 2003 5:59 pm
Location: Massachusetts, USA
Contact:

Re: ummm ,,,what happened??

Post by Tony Smith »

The temps are nice, even centigrade numbers converted to Fahrenheit, which become really strange numbers.

Tony
The tightrope between being strange and being creative is too narrow to walk without occasionally landing on both sides..." Scott Berkun
Haydo
Posts: 292
Joined: Fri Mar 14, 2003 9:55 am
Location: Eimeo, Qld., Australia
Contact:

Re: ummm ,,,what happened??

Post by Haydo »

Nice look you had going on there with the stringer. Would loved to have seen your face when it let go. If you keep pushing the boundaries with your work you'll get similar days. This site is where you'll build a strong foundation to work from. peace, haydo
Life is like a raft, so be like a rat!...Challenging being a captain type rat though, going down with each ship and all!!