Iridized Bumps or Bubbles

This is the main board for discussing general techniques, tools, and processes for fusing, slumping, and related kiln-forming activities.

Moderators: Brad Walker, Tony Smith

Post Reply
NinaMiller
Posts: 4
Joined: Thu Aug 07, 2014 9:24 pm

Iridized Bumps or Bubbles

Post by NinaMiller »

I am having trouble full fusing black backed iridized rainbow glass. If I use any pieces bigger than 2 inches square I get bumps. I assumed that meant I needed a slower schedule so I switched to one that was supposed to be a bubble squeeze. Still getting bumps. I'm also getting bumps in streakies. No problems with regular opaques or transparents. I just started fusing in my own kiln. First used the presets. Then went to Slumpy's schedules. Now scouring the web...
Attachments
Here is a photo of the bumps. The line that looks kind of like a crack is actually a piece of vitrigraph so ignore that.
Here is a photo of the bumps. The line that looks kind of like a crack is actually a piece of vitrigraph so ignore that.
Brad Walker
Site Admin
Posts: 1543
Joined: Fri Mar 07, 2003 9:33 pm
Location: North Carolina, USA
Contact:

Re: Iridized Bumps or Bubbles

Post by Brad Walker »

What schedule are you using? What brand of glass?
NinaMiller
Posts: 4
Joined: Thu Aug 07, 2014 9:24 pm

Re: Iridized Bumps or Bubbles

Post by NinaMiller »

This is bullseye glass. Here's the latest schedule I've tried:
400 1000 20
400 1150 15
50 1250 20
850 1450 15
Afap 950 60
400 100 0

Another schedule used:
300 1150 30
200 1370 20
400 1480 20
Afap 950 60
150 800 10
300 100 0

Interestingly i took a small piece off another bumpy plate and full fused it again. Most bumps disappeared. Then when I slumped it all the bumps disappeared. 3 inches square. Large piece with 2 inch squares from this same sheet fused fine.
JestersBaubles
Posts: 705
Joined: Fri Feb 25, 2011 12:01 am
Location: North Logan, UT
Contact:

Re: Iridized Bumps or Bubbles

Post by JestersBaubles »

NinaMiller wrote:This is bullseye glass. Here's the latest schedule I've tried:
400 1000 20
400 1150 15
50 1250 20
850 1450 15
Afap 950 60
400 100 0

Another schedule used:
300 1150 30
200 1370 20
400 1480 20
Afap 950 60
150 800 10
300 100 0

Interestingly i took a small piece off another bumpy plate and full fused it again. Most bumps disappeared. Then when I slumped it all the bumps disappeared. 3 inches square. Large piece with 2 inch squares from this same sheet fused fine.
Depending upon the piece and the kiln, 20 minutes may not be a long enough bubble squeeze at 1250. Try 60 minutes -- seems to work well in my Skutt GM1414 (side and top elements).

Other thoughts:
You said you are using Bullseye Glass, but the anneal at 950 is a typical temp for System 96. Bullseye is 920 deg F
If you are fusing large pieces, or pieces that have been previously fired, a ramp of 400/hr on the way up to 1150 may be too quick. You could end up with thermal shock.

Dana W.