fill weight and firing schedule?

This is the main board for discussing general techniques, tools, and processes for fusing, slumping, and related kiln-forming activities.

Moderators: Brad Walker, Tony Smith

Post Reply
peterbr
Posts: 36
Joined: Tue Feb 24, 2004 8:36 pm

fill weight and firing schedule?

Post by peterbr »

Does anyone have a fill weight for each cast heart and a firing schedule for this casting mold?
Attachments
47140.jpg
47140.jpg (38.4 KiB) Viewed 9888 times
Judd
Posts: 295
Joined: Mon Sep 01, 2003 9:45 am
Location: Arkansas

Re: fill weight and firing schedule?

Post by Judd »

Are you wanting them all to be uniform? If not, I just fill until the glass is heaping over.
Peter McCarthy
Posts: 19
Joined: Wed Feb 22, 2006 10:48 am
Location: Cambridge, MA

Re: fill weight and firing schedule?

Post by Peter McCarthy »

Glass weighs 2.5 times as much as water. Weigh the amount of water that fills a heart and multiply by 2.5 for the amount of glass needed.
Brad Walker
Site Admin
Posts: 1543
Joined: Fri Mar 07, 2003 9:33 pm
Location: North Carolina, USA
Contact:

Re: fill weight and firing schedule?

Post by Brad Walker »

Peter McCarthy wrote:Glass weighs 2.5 times as much as water. Weigh the amount of water that fills a heart and multiply by 2.5 for the amount of glass needed.
Alternatively, just fill the mold and fire. Weigh the finished piece. If it's too big, subtract some frit next time. If it's too small, add some frit.

The firing schedule is more or less a normal full fuse with a slightly longer hold at the top and a longer anneal time.
Post Reply