mine: for three layer 71/2 x 11 assembled frit sheets. which works
300 1215 2.00
100 1490 :20
9999 910 2:00
100 750 .15
However I am now doing four layers of 12x12 assembled frit sheets. Do you think I need to change this schedule at all. Thank you for any advice, I'm really bad at changing schedules that I know work.
firing schedule
Moderators: Brad Walker, Tony Smith
-
The Hobbyist
- Posts: 311
- Joined: Sun Mar 09, 2003 7:09 pm
- Location: Sun City West (NW Phoenix), AZ
- Contact:
Re: firing schedule
I would add/change 50 800 to the anneal for this one and the next.