Screen melt bubbles

This is the main board for discussing general techniques, tools, and processes for fusing, slumping, and related kiln-forming activities.

Moderators: Brad Walker, Tony Smith

Post Reply
michelletallin
Posts: 3
Joined: Mon Mar 30, 2020 6:41 pm

Screen melt bubbles

Post by michelletallin »

Hi, I've been fusing for a few years but I am new to pot/screen melting and with my second attempt I've ended up with holes, presumably from bubbles forming.
What do I need to do to resolve this? I presume I need to tweak the firing schedule?
I'm using the attached schedule
Many thanks,
Michelle
Attachments
IMG_1411.jpg
schedule.JPG
JestersBaubles
Posts: 705
Joined: Fri Feb 25, 2011 12:01 am
Location: North Logan, UT
Contact:

Re: Screen melt bubbles

Post by JestersBaubles »

Looks to me like you need more glass.

Dana W.
Brad Walker
Site Admin
Posts: 1544
Joined: Fri Mar 07, 2003 9:33 pm
Location: North Carolina, USA
Contact:

Re: Screen melt bubbles

Post by Brad Walker »

JestersBaubles wrote:Looks to me like you need more glass.
I was thinking the same thing.
michelletallin
Posts: 3
Joined: Mon Mar 30, 2020 6:41 pm

Re: Screen melt bubbles

Post by michelletallin »

Thanks - I'll try again!
michelletallin
Posts: 3
Joined: Mon Mar 30, 2020 6:41 pm

Re: Screen melt bubbles

Post by michelletallin »

You were absolutely right, wont make that mistake again!
I refired with some extra glass and it actually came out pretty good
Thank you!