I was casting something and the mold poured out onto kiln shelf and the heating elements. I have about 6mm thick glass encasing some of the heating coils.
I chisseled off some chunks, but I'm. afraid of doing damage to the kiln if repeatdely pounding. should I heat up to 500 degrees and glass cool it, would that remove the glass better?
melted mess
Moderators: Brad Walker, Tony Smith
-
Brad Walker
- Site Admin
- Posts: 1543
- Joined: Fri Mar 07, 2003 9:33 pm
- Location: North Carolina, USA
- Contact:
Re: melted mess
I've had a situation where the glass remained on the coils for years, so that would be my first choice. Do nothing until you eventually need to change the elements.
If anyone else has a better solution, love to hear it.
If anyone else has a better solution, love to hear it.
-
Michael Stevens
- Posts: 83
- Joined: Thu Dec 26, 2019 2:52 pm
Re: melted mess
So I removed some of the glass, opened the coils a little and then put back in place. I'm testing it now , if I screwed the coils, I can get replaced for less than 200 dollars, not too bad, . but I'm hopeful this will be ok
-
jim simmons
- Posts: 478
- Joined: Sun Mar 09, 2003 10:37 pm
- Location: Hillsboro Oregon
- Contact:
Re: melted mess
Should e just fine, I did exactly what Brad did about 6 years ago and it is working just fine.
The other Jim
The other Jim
-
Kevin Midgley
- Posts: 774
- Joined: Mon Mar 10, 2003 11:36 am
- Location: Tofino, British Columbia, Canada
Re: melted mess
I had glass on elements for years.
If you have some electrical safety controls, turn off, remove power when kiln is heated to say 800F???
With a spray bottle of water dialed to a fine stream, Open the kiln and spray onto the glass which if you are lucky will crack from the thermal shock and become removable.
allow kiln to cool and remove glass carefully.
Repeat as needed but also do at your own risk.
If you have some electrical safety controls, turn off, remove power when kiln is heated to say 800F???
With a spray bottle of water dialed to a fine stream, Open the kiln and spray onto the glass which if you are lucky will crack from the thermal shock and become removable.
allow kiln to cool and remove glass carefully.
Repeat as needed but also do at your own risk.