I'm. making a 30 inch x 40 inch 9mm thick panel what should the anneal time be? I thought about 12 hours would that be enough
-
Brad Walker
- Site Admin
- Posts: 1544
- Joined: Fri Mar 07, 2003 9:33 pm
- Location: North Carolina, USA
- Contact:
Re: annealling large panels
Bullseye would say about half that, or less. http://www.bullseyeglass.com/methods-id ... slabs.html
They don't have 9mm in their chart, so to be conservative go with 12mm or even 19mm, which are still below 12 hours.
They don't have 9mm in their chart, so to be conservative go with 12mm or even 19mm, which are still below 12 hours.
-
Bert Weiss
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
Re: annealling large panels
I anneal 10mm float with a 1.2 hour soak at 1000, 1.2 hours down to 900, .8 hours down to 700, .8 hours down to 300. For fusing glasses, I drop those temps down 80ºF. A twelve hour soak would insure the glass would be the same as the kiln, from edge to edge. In most kilns that would insure annealing impossibility. You really can anneal soak too long. The temperature near the walls isn’t the same as in the center. Annealing actually takes place in about 15 seconds when the entire mass of glass is within 5ºC inside the annealing range, no matter what size the glass is.Michael Stevens wrote:I'm. making a 30 inch x 40 inch 9mm thick panel what should the anneal time be? I thought about 12 hours would that be enough
If our thickness isn’t uniform, I might extend to 2 hours soak, from 1.2 etc.
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions