fusing

This is the main board for discussing general techniques, tools, and processes for fusing, slumping, and related kiln-forming activities.

Moderators: Brad Walker, Tony Smith

Post Reply
Bruce
Posts: 14
Joined: Tue Apr 15, 2003 9:37 pm

fusing

Post by Bruce »

I am new to fusing and am having a hard time getting two pieces to fuse
all the way across. It usually fuses at the top and bottom and leaves a
gap in the middle. Do the pieces have to be perfectly touching to fuse?
I am taking it to 1450 degrees, do I need to go higher?
Brad Walker
Site Admin
Posts: 1542
Joined: Fri Mar 07, 2003 9:33 pm
Location: North Carolina, USA
Contact:

Post by Brad Walker »

You need to read the tutorial on this website: http://www.warmglass.com/Basic.htm
Jane Lindell
Posts: 29
Joined: Mon Mar 10, 2003 5:36 pm
Location: Marion, Iowa
Contact:

Post by Jane Lindell »

Are you using only 1 layer of glass?

Glass naturally wants to be 1/4" thick - so if there is only one 1/8" layer (or gaps in the top layer) it will "pull" in and try to become 1/4" thick.

Most people commonly use a solid piece of glass for the bottom layer and then put the design pieces on top. Yes, you need to cut precisely and have the edges touching to get the edges to fuse together.

Hope this helps.
Bruce
Posts: 14
Joined: Tue Apr 15, 2003 9:37 pm

Post by Bruce »

Thanks,
I did not realize that glass wanted to be 1/4 inch. I will try again using
two layers. So far I have some interesting sun catchers so all is not lost.
Bruce
Bruce
Posts: 14
Joined: Tue Apr 15, 2003 9:37 pm

Post by Bruce »

Thanks again,
Finally got something to fuse like I wanted. From now on its two pieces of glass stacked.
PaulS
Posts: 155
Joined: Mon Mar 10, 2003 6:45 pm
Location: Belize
Contact:

Post by PaulS »

Jane Lindell wrote:Are you using only 1 layer of glass?

Most people commonly use a solid piece of glass for the bottom layer and then put the design pieces on top. Yes, you need to cut precisely and have the edges touching to get the edges to fuse together.
and some people put the design elements on the bottom with a panel of clear on top, like this;
Image

That way it gives depth and a shiney smooth top surface.

Cut the top (clear layer) big enough to overlap the base. The amount of overlap is the same as the thickness of the base.

Just another option for you to consider.

Paul