Eureka
Moderators: Brad Walker, Tony Smith
- 
				Steve Immerman
- Posts: 208
- Joined: Sun Mar 09, 2003 4:55 pm
- Location: Eau Claire, Wisconsin
- Contact:
Eureka
Well, I think I've solved the hazy irid sandwich problem. In short, it's the silicon carbide grit.
After innumerable failures with silicon carbide (both 120 and 220 grit), I changed the grit in my blaster to 120 aluminum oxide and blasted, cleaned and fired the same way I had been.
Came out perfect. The difference in appearance between using the two blasting mediums is dramatic.
I also, blasted and firepolished some pieces, including deep purple transparent, black, and clear. They also came out looking better than the ones I blasted and firepolished with the silicon carbide. Less little tiny pits on the surface.
So, I would question the conventional wisdom that these abrasives are interchangeable when used for glass fusing.
Steve
ps. anybody want to buy some almost-new silicon carbide grit?
			
			
									
						
										
						After innumerable failures with silicon carbide (both 120 and 220 grit), I changed the grit in my blaster to 120 aluminum oxide and blasted, cleaned and fired the same way I had been.
Came out perfect. The difference in appearance between using the two blasting mediums is dramatic.
I also, blasted and firepolished some pieces, including deep purple transparent, black, and clear. They also came out looking better than the ones I blasted and firepolished with the silicon carbide. Less little tiny pits on the surface.
So, I would question the conventional wisdom that these abrasives are interchangeable when used for glass fusing.
Steve
ps. anybody want to buy some almost-new silicon carbide grit?
- 
				Ron Coleman
- Posts: 468
- Joined: Sun Mar 09, 2003 3:20 pm
- Location: Columbus, Ohio USA
Re: Eureka
Good going Steve. Nice to have one that works.Steve Immerman wrote:Well, I think I've solved the hazy irid sandwich problem. In short, it's the silicon carbide grit.
After innumerable failures with silicon carbide (both 120 and 220 grit), I changed the grit in my blaster to 120 aluminum oxide and blasted, cleaned and fired the same way I had been.
Came out perfect. The difference in appearance between using the two blasting mediums is dramatic.
I also, blasted and firepolished some pieces, including deep purple transparent, black, and clear. They also came out looking better than the ones I blasted and firepolished with the silicon carbide. Less little tiny pits on the surface.
So, I would question the conventional wisdom that these abrasives are interchangeable when used for glass fusing.
Steve
ps. anybody want to buy some almost-new silicon carbide grit?
It sure would be interesting to see a microscopic view of the surfaces created by the two different blasting media. This one is weird for sure. Either surface contamination from the media or a difference in the blasted texture.
Ron
- 
				Steve Immerman
- Posts: 208
- Joined: Sun Mar 09, 2003 4:55 pm
- Location: Eau Claire, Wisconsin
- Contact:
Ron,
My theory is it is the texture of the blasted surface. I was going to see if one of my friends has one of those Intel digital microscopes that connects to the USB port of the computer and compare the surfaces- but now the silicon carbide is out of the blaster, and it's a real project to put it back in.
Steve
			
			
									
						
										
						My theory is it is the texture of the blasted surface. I was going to see if one of my friends has one of those Intel digital microscopes that connects to the USB port of the computer and compare the surfaces- but now the silicon carbide is out of the blaster, and it's a real project to put it back in.
Steve
Nikki and the Microscope
I had the honor of visiting Nikki O'Neill's fungus laboratory last week, and there was this very new and very amazing microscope . . .  (also a neat antique one).
If someone would send her two small samples (silicon carbide and aluminum oxide), bet she could get the differences in a photo and post them.
(Nikki, if this happens, can I come see?)
Beth
P.S. For you magneteers, Nikki's was the detailed pate de verre leaf with spirit face. . .
			
			
									
						
										
						If someone would send her two small samples (silicon carbide and aluminum oxide), bet she could get the differences in a photo and post them.
(Nikki, if this happens, can I come see?)
Beth
P.S. For you magneteers, Nikki's was the detailed pate de verre leaf with spirit face. . .
- 
				Pam Hrycyk
- Posts: 36
- Joined: Mon Mar 10, 2003 9:17 pm
- Location: Toronto, Ontario Canada
Re: Eureka
Steve, I'm glad you figured out the problem but now I'll be worried about Brock's Pilchuck auction piece. He posted earlier that he was in the middle of it and used silicon carbide to blast.Steve Immerman wrote:Well, I think I've solved the hazy irid sandwich problem. In short, it's the silicon carbide grit.
After innumerable failures with silicon carbide (both 120 and 220 grit), I changed the grit in my blaster to 120 aluminum oxide and blasted, cleaned and fired the same way I had been.
Came out perfect. The difference in appearance between using the two blasting mediums is dramatic.
Pam
- 
				Barbara Muth
- Posts: 382
- Joined: Sun Mar 09, 2003 8:10 pm
- Location: Washington DC Metropolitan Area
- Contact:
Maybe Tony could supply the silicon carbide surfce. I would love to see the difference. Glad you solved things Steve, this should add a lot to your upcoming work! i'll be sneaking a peek at your website.Steve Immerman wrote:Ron,
My theory is it is the texture of the blasted surface. I was going to see if one of my friends has one of those Intel digital microscopes that connects to the USB port of the computer and compare the surfaces- but now the silicon carbide is out of the blaster, and it's a real project to put it back in.
Steve
Barbara
- 
				Steve Immerman
- Posts: 208
- Joined: Sun Mar 09, 2003 4:55 pm
- Location: Eau Claire, Wisconsin
- Contact:
Re: Eureka
Pam,Pam Hrycyk wrote:
Steve, I'm glad you figured out the problem but now I'll be worried about Brock's Pilchuck auction piece. He posted earlier that he was in the middle of it and used silicon carbide to blast.
Pam
I don't have a good feeling about his piece either.....
Steve
ps you should be getting something from me in the mail soon.
- 
				Pam Hrycyk
- Posts: 36
- Joined: Mon Mar 10, 2003 9:17 pm
- Location: Toronto, Ontario Canada
- 
				Nikki ONeill
- Posts: 169
- Joined: Mon Mar 10, 2003 11:55 am
- Location: Silver Spring, MD
- Contact:
I'd be thinking how neat neat it'd be to see the difference betweent he effects of the two abrasives up c.ose (thanks for the prompt, Beth).  If anyone want would like to see a photo, I'll take a look and photograph the samples with a digital stereomicroscope.  My bigger compound microscope is not yet wet up yet, but will be soon.  I'm sure we'll be able to see some differences with the dissecting scope.  So if anyone would like to send a couple of samples, e-mail me and I'll send you my address.  The images in this year's copy of the Nikon microscope calendar are amazing and may be of interest to some.  You may be able to get a copy by request on-line...I'll check and post later. Nikki
			
			
									
						
										
						- 
				Nikki ONeill
- Posts: 169
- Joined: Mon Mar 10, 2003 11:55 am
- Location: Silver Spring, MD
- Contact:
- 
				Glenda Kronke
- Posts: 64
- Joined: Tue Mar 11, 2003 11:44 am
- Location: Austin, TX
- Contact:
I have one of those Nikon calendars from about 10 years back and it is one of my favorites! It had photos of contest results.   PLEASE let me know how to get another one! The microscopic photos of different elements and things is facinating! I am even trying to duplicate some of them in fused glass with some interesting results.  A couple of months ago I did a search in 'google' tm but can't find the site now.  It was incredible and great inspiration!  Maybe on of you guys that is a search wiz can find it and post it?
glenda
			
			
									
						
										
						glenda
- 
				Glenda Kronke
- Posts: 64
- Joined: Tue Mar 11, 2003 11:44 am
- Location: Austin, TX
- Contact:
OT/Microscope photos
Sorry, I know this should probably go in the 'Spab' location- Thanks Nikki for the link to website (see silicon carbide vs aluminum oxide results). My calendar was from 1992 and I have been trying to duplicate 18th prize in glass. It nature beautiful!  *Will direct any additional comments to Spab. Sorry
glenda
			
			
									
						
										
						glenda
- 
				Tony Smith
- Posts: 1037
- Joined: Sun Mar 09, 2003 5:59 pm
- Location: Massachusetts, USA
- Contact:
I'd be more than happy to supply the silicon carbide blasted sample... just let me know what the parameters are (glass type, color, pressure, nozzle diameter, grit size, etc...). It may take me a week or two to get to it since I'll be out of town for the next week and a half.
Tony
			
			
									
						
							Tony
The tightrope between being strange and being creative is too narrow to walk without occasionally landing on both sides..."   Scott Berkun
			
						- 
				Steve Immerman
- Posts: 208
- Joined: Sun Mar 09, 2003 4:55 pm
- Location: Eau Claire, Wisconsin
- Contact:
- 
				Nikki ONeill
- Posts: 169
- Joined: Mon Mar 10, 2003 11:55 am
- Location: Silver Spring, MD
- Contact:
Tony and Steve:
Off the top of my head, black would probably be better to see fracture differences, but it could be incredibly beautiful to see what the glass it would look like in clear. (The scopes are equipped with reflected and transmitted light, as well as Nomarski, i.e.polarized, optics). There might be lots of light reflections. When you get a chance, send a couple of labeled samples and I'll see what I can do. I'll be in Roger Thomas's class at Vitrum this weekend and might get a chance ato make a couple of aluminum oxide samples from Judy and Kevin's blaster.
Nikki
			
			
									
						
										
						Off the top of my head, black would probably be better to see fracture differences, but it could be incredibly beautiful to see what the glass it would look like in clear. (The scopes are equipped with reflected and transmitted light, as well as Nomarski, i.e.polarized, optics). There might be lots of light reflections. When you get a chance, send a couple of labeled samples and I'll see what I can do. I'll be in Roger Thomas's class at Vitrum this weekend and might get a chance ato make a couple of aluminum oxide samples from Judy and Kevin's blaster.
Nikki
- 
				Nikki ONeill
- Posts: 169
- Joined: Mon Mar 10, 2003 11:55 am
- Location: Silver Spring, MD
- Contact:
- 
				Brad Walker
- Site Admin
- Posts: 1537
- Joined: Fri Mar 07, 2003 9:33 pm
- Location: North Carolina, USA
- Contact:
I'm going to be very interested in these results also, although I'm not sure how much credence to give these simple tests. We have had problems using SiC, but we've also used it successfully. We've never this kind of problem with AlOx. To me, fire polishing is fire polishing, and all marks should be gone, unless it's a cleaning issue. I have, many times, fire polished glass with blasting and dremelling with perfect results.  Brock
			
			
									
						
							My memory is so good, I can't remember the last time I forgot something . . .
			
						- 
				Nikki ONeill
- Posts: 169
- Joined: Mon Mar 10, 2003 11:55 am
- Location: Silver Spring, MD
- Contact:
Brock:  I'm sure we'll get something out of it, even if it's knowing how many fractures can fit on the pinnicle of a silicon carbide fragment. (good mag question??)  Not really knowing much, you'd think that any flameworked surface would look similar.  What we're not controlliing for is the length of the blasting time and the age (particle size) of the silicone carbide, both of which may affect surface structure of the blasted sample.  But we're getting into a thesis project here, and this is supposed to be art. as has been said.   
 
Have a great weekend.
Nikki
			
			
									
						
										
						 
 Have a great weekend.
Nikki