Fusing went funky
Moderators: Brad Walker, Tony Smith
-
Dee Newbery
- Posts: 11
- Joined: Thu May 01, 2003 12:34 pm
- Location: Topeka, KS
Fusing went funky
I'm stumped. Have been trying different fusing schedules with my new kiln and am beginning to feel I don't know anything about fusing. I've had some real unhappy results.
The latest:
A elongated, rectangle 14" long, 4 1/4" at one end and 6 1/2" at the other.
It's a mask comprised of a clear dbl rl base, with interlocking pieces of opal on top, and additional pieces of opal, confetti, rod, stringer and frit sprinkled about. I fused this using the schedule below which I thought was slow enough to eliminate any bubbles. However, the face looks like it has pimples everywhere there is the single layer of opal.
This is all BE glass fired on thin fire shelf paper.
Can anyone suggest what happened? Also is it possible to refuse this to get rid of the pimples, if so what temps, etc?
400 dpm to 1180 - soak 30min
500 dpm to 1450 - soak 0
9999 to 960 - soak 1 hr.
210 dpm to 750 - soak 0
9999 to 80 - soak 0
another question - everyone talks about watching and checking the glass fuse and/or slump. How do you do that - don't you risk thermal shock when you open the door even briefly?
D
The latest:
A elongated, rectangle 14" long, 4 1/4" at one end and 6 1/2" at the other.
It's a mask comprised of a clear dbl rl base, with interlocking pieces of opal on top, and additional pieces of opal, confetti, rod, stringer and frit sprinkled about. I fused this using the schedule below which I thought was slow enough to eliminate any bubbles. However, the face looks like it has pimples everywhere there is the single layer of opal.
This is all BE glass fired on thin fire shelf paper.
Can anyone suggest what happened? Also is it possible to refuse this to get rid of the pimples, if so what temps, etc?
400 dpm to 1180 - soak 30min
500 dpm to 1450 - soak 0
9999 to 960 - soak 1 hr.
210 dpm to 750 - soak 0
9999 to 80 - soak 0
another question - everyone talks about watching and checking the glass fuse and/or slump. How do you do that - don't you risk thermal shock when you open the door even briefly?
D
-
Cynthia
Re: Fusing went funky
Assuming your frit and stringers are on top and not sandwiched, I'd say your schedule is a good bubble reducing schedule. I ramp up to 1150 with no soak and then creep up to 1250 at 60 -100 dph, then ramp at 500 dph to full fuse. Best bubble reducing schedule I've got. Learned it from a post by Lynne Chappell.Dee Newbery wrote:I'm stumped. Have been trying different fusing schedules with my new kiln and am beginning to feel I don't know anything about fusing. I've had some real unhappy results.
The latest:
A elongated, rectangle 14" long, 4 1/4" at one end and 6 1/2" at the other.
It's a mask comprised of a clear dbl rl base, with interlocking pieces of opal on top, and additional pieces of opal, confetti, rod, stringer and frit sprinkled about. I fused this using the schedule below which I thought was slow enough to eliminate any bubbles. However, the face looks like it has pimples everywhere there is the single layer of opal.
This is all BE glass fired on thin fire shelf paper.
Can anyone suggest what happened? Also is it possible to refuse this to get rid of the pimples, if so what temps, etc?
400 dpm to 1180 - soak 30min
500 dpm to 1450 - soak 0
9999 to 960 - soak 1 hr.
210 dpm to 750 - soak 0
9999 to 80 - soak 0
another question - everyone talks about watching and checking the glass fuse and/or slump. How do you do that - don't you risk thermal shock when you open the door even briefly?
D
If I misunderstood, and you sandwiched some glass bits between the base and the top, then your pimples are from the air you trapped.
As far as losing the acne...I've never had much success (with glass or skin
You risk thermal shocking the glass at temps below 1000F. If you peek above that temp, your glass will be fine...but no peeking at lower than that 'til it's cool.
-
Strega
But I looked at a piece I did last night with gold BE rainbow on the bottom and orange on the top with chunks of other colors.
So I'm thinkin' the surface of the irid glass is rough. That's how it reflects light the way it does. But it didn't do this on the other pieces which are other colors, even the big bowl I did that was a sandwitch of purple opal and white opal.
Maybe you should call up/email Bullseye....
there's an old batch of be wash that can cause this. it's a chemical interaction between the irid and the wash that produces the gasses that cause the bubbles. it appears as a spongy effect on the irid side of the glass.Strega wrote: But I looked at a piece I did last night with gold BE rainbow on the bottom and orange on the top with chunks of other colors.The thing is full of trapped bubbles on one half. None of my other pieces have this. my partner, who is a glass blower and all round science guy, said that to him it looks, not like the air trapped between layers and frit, which is the usual case with bubbles, but like it came all the way up from the bottom surface of the irid. Trapped air between the irid and the shelf.
So I'm thinkin' the surface of the irid glass is rough. That's how it reflects light the way it does. But it didn't do this on the other pieces which are other colors, even the big bowl I did that was a sandwitch of purple opal and white opal.Maybe this is batch specific?
Maybe you should call up/email Bullseye....
-
gone
You can also get this with BE silver irrid and thinfire.charlie wrote:there's an old batch of be wash that can cause this. it's a chemical interaction between the irid and the wash that produces the gasses that cause the bubbles. it appears as a spongy effect on the irid side of the glass.Strega wrote: But I looked at a piece I did last night with gold BE rainbow on the bottom and orange on the top with chunks of other colors.The thing is full of trapped bubbles on one half. None of my other pieces have this. my partner, who is a glass blower and all round science guy, said that to him it looks, not like the air trapped between layers and frit, which is the usual case with bubbles, but like it came all the way up from the bottom surface of the irid. Trapped air between the irid and the shelf.
So I'm thinkin' the surface of the irid glass is rough. That's how it reflects light the way it does. But it didn't do this on the other pieces which are other colors, even the big bowl I did that was a sandwitch of purple opal and white opal.Maybe this is batch specific?
Maybe you should call up/email Bullseye....
Els
-
kelly alge
- Posts: 81
- Joined: Sun Mar 09, 2003 8:31 pm
- Location: Findlay, OH
- Contact:
-
Strega
I think it looks interesting in the piece I did--the bubbles didn't come to the surface but are trapped. However, it is currently flat; I am planning to "drop ring" it so the result might not be good. It's all an experiment.kelly alge wrote:Do you have photos of this? Is this really ugly, or could you use this as a design element? Is it possible to make it happen regularly?
full-of-questions-girl
Speaking of photos, I haven't gotten the hang of THAT yet...I want to post requesting help on that but don't know which bulletin board to use....
-
kelly alge
- Posts: 81
- Joined: Sun Mar 09, 2003 8:31 pm
- Location: Findlay, OH
- Contact:
-
Strega
-
Lynne Chappell
- Posts: 186
- Joined: Fri Mar 14, 2003 2:05 am
- Location: Surrey B.C. Canada
- Contact:
I use a lot of black and even little bubbles look really awful if they are raised on the surface. As well as going really slow from 1150 to 1250, I have found that I will have small "pimples" at 1450, but if I fire a little higher (to 1480) they somehow flatten out. It's like the glass levels out around the bubbles and it looks much better. This doesn't fix the BIG bubbles, just the slight irregularity in the surface from little bubbles. You might try refiring a little hotter and see if it works for you.
I look in my kiln all the time. You do need to be careful at lower (slumping) temperatures. In my Clamshell the whole kiln lifts up and the glass is really exposed to chill. I did crack one piece cause I couldn't see the other side of the form and had the lid open for a bit too long. I've never cracked one in the top loading kiln. But don't hold it open too long when you're only slumping. And I NEVER open the kiln under 1100F. Even if I heard the dreaded ping, I still wait until it gets up to 1100 before I peek in to see if I need to start all over.
I look in my kiln all the time. You do need to be careful at lower (slumping) temperatures. In my Clamshell the whole kiln lifts up and the glass is really exposed to chill. I did crack one piece cause I couldn't see the other side of the form and had the lid open for a bit too long. I've never cracked one in the top loading kiln. But don't hold it open too long when you're only slumping. And I NEVER open the kiln under 1100F. Even if I heard the dreaded ping, I still wait until it gets up to 1100 before I peek in to see if I need to start all over.
-
kelly alge
- Posts: 81
- Joined: Sun Mar 09, 2003 8:31 pm
- Location: Findlay, OH
- Contact:
Yikes, I'm doing it!woo hoo, is this 0124 red?Dani wrote:Kelly, you have to start now or your baby will be telling you how to do this! Click the "quote" button in the top right corner of this post and say hi to me in the next post!Then figure out how to change the colors of the font and let me know....
thanks Dani!
kelly alge