putting a rim on a pot drop.

This is the main board for discussing general techniques, tools, and processes for fusing, slumping, and related kiln-forming activities.

Moderators: Brad Walker, Tony Smith

Post Reply
deborahbur
Posts: 51
Joined: Thu Apr 10, 2003 2:09 pm
Location: Tiverton, Rhode Island
Contact:

putting a rim on a pot drop.

Post by deborahbur »

Help
I still don't understand how to put a rim on a pot drop. Have read, but don't comprehend.

Do you cut a large circle and put your pot drop on top and then cut another circle with a hole the size of the drop?

Thanks
Deborah 8)
Brad Walker
Site Admin
Posts: 1543
Joined: Fri Mar 07, 2003 9:33 pm
Location: North Carolina, USA
Contact:

Post by Brad Walker »

Read this: it covers both circles and rims: http://www.system96.com/Pages/CircleDemo/Circle1.html
Steve Immerman
Posts: 208
Joined: Sun Mar 09, 2003 4:55 pm
Location: Eau Claire, Wisconsin
Contact:

Post by Steve Immerman »

I have only done this once, but learned quite a bit in the process.

First, I would recommend making a 3mm thick circle the diameter you want for your finished piece.

Then, grind the pot melt into a perfect circle.

Then cut one or two rims (depending on the thickness of the melt) as in Patty Gray's tutorial that Brad indicated. Make the inside rim about 1/8" larger in diameter than the pot melt.

Place the melt in the center of the blank with the rim (or rims) around the melt.

Fire to full fuse.

Hope this helps

Steve


Image
deborahbur
Posts: 51
Joined: Thu Apr 10, 2003 2:09 pm
Location: Tiverton, Rhode Island
Contact:

glass rims

Post by deborahbur »

Thanks, now I get it. Couldn't find Patty Gray's tutorial and your explanation is very simple.
Post Reply