Drop Out Mold

Posted: Sat Nov 01, 2003 12:24 am
by Mare
I'm doing my first drop out slump. I have 3 layers of Bullseye all fired and ready for the slump. Can someone clue me in as to a schedule for this? thanks.. :wink:

Re: Drop Out Mold

Posted: Sat Nov 01, 2003 1:55 pm
by jim simmons
Mare wrote:I'm doing my first drop out slump. I have 3 layers of Bullseye all fired and ready for the slump. Can someone clue me in as to a schedule for this? thanks.. :wink:
I use.
625 to 1275
hold for 30 min.
afap to 1380
hold until it looks right. About 15 min depending on the color of the glass.
anneal for 3 layers

Jim