At what temp should I fuse various wine bottles to flatten them to make a cheese tray, and how long do they need to anneal? Need info asap.
Thanks
camaro
Posted: Fri Mar 28, 2003 11:58 am
by rosanna gusler
in my kiln, 1530f does the job. i hold at 1030f for 20 min........ then 85 dph to 945.........then 165dph to 800f..then off. brick side fire ceramic kiln. rosanna
Posted: Fri Mar 28, 2003 12:34 pm
by Carol
I think there is a section on this in the FAQ.
Posted: Fri Mar 28, 2003 2:46 pm
by Cynthia
Camaro,
Here's the link to the tutorial.
http://www.warmglass.com/Bottles.htm
Having a wine and cheese party? Have fun regardless.

Posted: Fri Mar 28, 2003 8:49 pm
by Jeri D
]I am not so swift with bottles either
How do you keep them from rolling? I now have a glass dust pan because one rolled over the side a bit and have a big sculpture of 3 fused bottles. I guess you should do all the same bottles at once. Tried 2 kinds of vodka and blue glass.
Jeri,flunked bottles 101