I'm trying to tack fuse stringers on a piece and it's not going well. 
I want to create a design made of 1mm black stringers on top of a previously full fused piece. The placement of the stringers must be very precise for the design to work. However, even though I've glued them down (glass tack), they keep moving once the kiln starts to heat up.
Is there some way to keep the stringers in place until they are fused?
I'm still farily new to fusing, so any suggestions would be greatly appreciated.
Happy New Year.
			
			
									
						
										
						I want to create a design made of 1mm black stringers on top of a previously full fused piece. The placement of the stringers must be very precise for the design to work. However, even though I've glued them down (glass tack), they keep moving once the kiln starts to heat up.
Is there some way to keep the stringers in place until they are fused?
I'm still farily new to fusing, so any suggestions would be greatly appreciated.
Happy New Year.
- 
				Lisa Allen
- Posts: 212
- Joined: Sun Mar 09, 2003 3:23 pm
- Location: Memphis, TN
- Contact:
You can also put sharpie marks where you want the stringers, then take a dremel with a diamond tipped bit to make little channels.
Lisa
			
			
									
						
							Lisa
Lisa Allen
http://www.lisa-allen.com
Today's mighty oak is just yesterday's nut that held its ground.
			
						http://www.lisa-allen.com
Today's mighty oak is just yesterday's nut that held its ground.
- 
				Rick Wilton
- Posts: 273
- Joined: Sat Oct 25, 2003 8:18 pm
- Location: Calgary, Canada
- Contact:
- 
				Patty Gray
- Posts: 70
- Joined: Mon Mar 10, 2003 9:47 pm
- Location: Washington
- Contact:
An easy way to have the stringer flat on the bottom is to put them into the kiln on a kilnwashed shelf (by themselves) and just go to a tack fuse firing.  It will flatten the bottom then they will not move around.  
Good luck.
Patty
http://www.pattygray.com
			
			
									
						
										
						Good luck.
Patty
http://www.pattygray.com
- 
				Mary Kay Nitchie
- Posts: 21
- Joined: Mon Mar 10, 2003 8:02 pm
- Location: Portland, Oregon
- Contact:
Good Ideas
I'll try creating a flat surface on the stringers, which sounds fairly easy to do. If that doesn't work, creating a channel seems like a sure thing. 
Thanks to everyone for the advice.
Ted
			
			
									
						
										
						Thanks to everyone for the advice.
Ted
 It easy !  You just have to watch the pressure cause boy they break easily.  I still glue them in place too