Page 1 of 1
					
				How o you prevent shrinkage oF the base glass when fusing?
				Posted: Thu Feb 12, 2004 4:56 pm
				by Helena
				When fusing large pieces of glass together, how do you prevent the base glass from shrinking up in various points along the edge?
			 
			
					
				
				Posted: Thu Feb 12, 2004 5:04 pm
				by charlie
				if it's 2 layers (1/4") it shouldn't shrink. if it's less, then it will. not much you can do about it. going slowly may help the matters, but probably won't eliminate it.
			 
			
					
				
				Posted: Thu Feb 12, 2004 7:31 pm
				by Geri Comstock
				Are you grinding the edges before you fuse?  If not, you may have areas where there's only 1 layer of glass and that will shrink up to its equilibrium thickness.
Are you firing too high?  This will leave sharpies on the edges.
Geri
			 
			
					
				
				Posted: Thu Feb 12, 2004 11:30 pm
				by Stuart Clayman
				Is the bottom layer Irid?