				firing schedule BE
				Posted: Thu Jul 03, 2014 9:33 pm
				by Andrea R
				I have never uesed this schedule before just thought I would run it pass all of you. Its BE full fuse for 2- 3mm glass. 
400 - 1225 - 30
600 - 1490 - 10
200 - 900 - 1:00
100 - 700 - 01
I have never gone that hot or that fast so 600 to 1490 seems so hot to me and is the 400-1225 30 min hold  long enough for a bubble squeeze ?
Fingers crossed  
 
Thanks
A
 
			 
			
					
				Re: firing schedule BE
				Posted: Fri Jul 04, 2014 12:12 pm
				by Drewcilla
				I do a lot of firing with enamel screen printing (kiln cured) on 3mm Tekta fired face down on 3mm glass.  This might be overkill for you but this schedule has worked very well for me:
300          1100         45
50            1250         1.00
400           1460         12
full            900           1.00
100           700           off
I put this schedule together from recommendations on this site.  I believe the top fusing temperature and hold is somewhat kiln specific.  I have a 14" Skutt Hotbox and 1460 works for me.  The biggest change I made and what seems to make a huge difference in terms of bubbles is the slow rise from 1100 to 1250 and the long hold at 1250.  This schedule has also been good when I'm going for a softer fuse (e.g. 1415).
Good luck,
Drewcilla
			 
			
					
				Re: firing schedule BE
				Posted: Fri Jul 04, 2014 12:46 pm
				by Andrea R
				happy to report it work like a charm...guess they know what there talking about at BE !