I want use red in a couple of wafers I'm making, but I haven't been able to get it to strike true red yet. I fired them up to 1285 the first time, 1300 the next. Still orange looking. I e-mailed BE and they told me it would only strike at full fusing temperatures but I've gotten red in wafers in the past, and I don't think it could have possibly been at full fuse temps. I don't want to just do a test run for two wafers, thought I'd ask here first. Learned my lesson--take better notes! Thanks!
Brad Walker
Site Admin
Posts: 1544
Joined: Fri Mar 07, 2003 9:33 pm
Location: North Carolina, USA
Contact:

Re: getting red to strike in a wafer

Post by Brad Walker »

My guess is that the red Bullseye makes today requires the higher temperature to fully strike, while the one they made in years past didn't. That's true of a lot of their colors, which tend to be sold as strikers where they used to be already struck (or at least partially struck) at the factory.

You might try a hold at around 1250F on the way up to see if that helps, but I don't think it will solve everything.
Kate Saunders
Posts: 53
Joined: Thu Mar 18, 2004 10:53 pm

Re: getting red to strike in a wafer

Post by Kate Saunders »

Hmmm....the red powder I am using is the same stuff I used on the original wafers (I buy the big jars). I'll just take a reject wafer and fire it with a regular load. Or e-mail the wafer master himself.
JestersBaubles
Posts: 705
Joined: Fri Feb 25, 2011 12:01 am
Location: North Logan, UT
Contact:

Re: getting red to strike in a wafer

Post by JestersBaubles »

Try 1325.

Dana W.
Babette (Shawn)
Posts: 103
Joined: Fri Feb 05, 2010 4:11 pm
Location: Chico California
Contact:

Re: getting red to strike in a wafer

Post by Babette (Shawn) »

What do you plan to do with your wafer?
“Art washes away from the soul the dust of everyday life.”
― Pablo Picasso
Morganica
Posts: 1079
Joined: Mon May 19, 2003 6:19 pm
Location: Portland, OR
Contact:

Re: getting red to strike in a wafer

Post by Morganica »

Which red?
Cynthia Morgan
Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery
http://www.cynthiamorgan.com

"I wrote, therefore I was." (me)
Kate Saunders
Posts: 53
Joined: Thu Mar 18, 2004 10:53 pm

Re: getting red to strike in a wafer

Post by Kate Saunders »

At 1340 the opal red powder finally turned red enough for my needs. I also tried pimento and tomato reds, which didn't strike very much at 1340. I'm using the wafer on top of glass that has had some powdered glass fired into it already, so the red and the white on the wafer has to be pretty dense. I'm building little glass houses, and the wafer will be part of the