Can I slump directly on a kiln shelf without a mold?

This is the main board for discussing general techniques, tools, and processes for fusing, slumping, and related kiln-forming activities.

Moderators: Brad Walker, Tony Smith

Post Reply
Marian P.
Posts: 8
Joined: Tue Sep 04, 2007 11:24 pm

Can I slump directly on a kiln shelf without a mold?

Post by Marian P. »

I'm pretty sure I can do this but thought I'd run it by "the experts". I have two large pieces to slump into an organic shape. I only have one mold and don't want to fire my big kiln half empty. So I was thinking about putting some fiber blanket under the parts I want to stay elevated and then just slumping the rest directly onto a kiln shelf. They are two large "coral" pieces so don't need much of a slump. Any reason I shouldn't do this?
Thanks!
Warren Weiss
Posts: 137
Joined: Thu Mar 13, 2003 8:06 pm
Location: Richmond, VA

Re: Can I slump directly on a kiln shelf without a mold?

Post by Warren Weiss »

No reason to not do it. Be sure there is some folded fiber blanket under the raised parts so that the blanket doesn't flatten out during the slump. Calculate your annealing time for the piece in the mold because it will cool slower than the piece over the fiber blanket.

Warren
Kevin Midgley
Posts: 774
Joined: Mon Mar 10, 2003 11:36 am
Location: Tofino, British Columbia, Canada

Re: Can I slump directly on a kiln shelf without a mold?

Post by Kevin Midgley »

uneven heating of the kiln shelf may result in it cracking. Cover half the shelf and watch it break. #-o
Judd
Posts: 295
Joined: Mon Sep 01, 2003 9:45 am
Location: Arkansas

Re: Can I slump directly on a kiln shelf without a mold?

Post by Judd »

I fire and slump on the floor of my kiln all the time.
1) Cover the floor with kiln wash (which you should do anyhow in case of an accident).
2) Extend your anneal time.
JestersBaubles
Posts: 705
Joined: Fri Feb 25, 2011 12:01 am
Location: North Logan, UT
Contact:

Re: Can I slump directly on a kiln shelf without a mold?

Post by JestersBaubles »

I have slumped platters where the two short edges are placed on fiber-paper covered kiln dams, and then allow the glass to slump to the kiln-washed or fiber-blanketed shelf.