When a color doesn't strike
Moderators: Brad Walker, Tony Smith
-
Laura Walter
- Posts: 6
- Joined: Mon Nov 22, 2004 2:58 pm
When a color doesn't strike
Can a color that didn't strike on the 1st time through the kiln (violet striker, #1234, came out a muddy transparent blue depending on the light) go through the kiln again to reach it's intended color or is it now scrap? I didn't hold it for 2 hours at 1225.
-
Brad Walker
- Site Admin
- Posts: 1543
- Joined: Fri Mar 07, 2003 9:33 pm
- Location: North Carolina, USA
- Contact:
Re: When a color doesn't strike
To help it strike better hold in the 1225 to 1240F range for half an hour one hour. Two hours is probably overkill.
-
Laura Walter
- Posts: 6
- Joined: Mon Nov 22, 2004 2:58 pm
Re: When a color doesn't strike
Thanks Brad.