Bubble

Post by Eric Bloom »

I'm sometimes getting a large bubble when fusing this piece, the long dimension is 12 inches. Fired on Papyros, my usual full-fuse program that works fine with smaller pieces, and sometimes works fine with this size. Any ideas what causes this?
IMG_4861.JPG
IMG_4862.JPG
Eric Bloom
Posts: 8
Joined: Fri May 15, 2020 3:39 pm

Re: Bubble

Post by Eric Bloom »

I think I found the answer ... right here on this website. I'll try adjusting my schedule.

https://warmglass.com/what-caused-this-huge-bubble/
Brad Walker
Site Admin
Posts: 1542
Joined: Fri Mar 07, 2003 9:33 pm
Location: North Carolina, USA
Contact:

Re: Bubble

Post by Brad Walker »

Eric Bloom wrote:I think I found the answer ... right here on this website. I'll try adjusting my schedule.

https://warmglass.com/what-caused-this-huge-bubble/
Yep. I was just about the send you that link. Slow down, reduce top temperature.