BE thinfire shelf paper
Moderators: Brad Walker, Tony Smith
BE thinfire shelf paper
I have a new kiln that has side heating elements in addition to elements on top. When I fire to full fuse using BE thinfire shelf paper, the paper splits underneath the glass. Also, if I leave extra paper around the sides of the glass, it folds over onto the top of the glass. My old kiln, which only had top elements never did this. Any idea why these things are happening?
-
Cynthia
The old thinfire - which is all I have ever used - shrinks.
You need to leave a good margin around your work, a couple of inches all around, and anchor it down with some small kiln furniture at the corners and mid way along the edges too dependent upon how large your surface is (bits scrap glass works too...just be sure it's a good 1/2" away from your piece, or it will get pulled into the work as the paper shrinks). For larger work, it's just going to tear underneath no matter what. At least I haven't figured out a way around it. You can sprinkle the surface of the paper with some talc or dry primer to allow the glass to glide as the paper shrinks, but it may still tear.
The new thinfire doesn't shrink. I don't know if it curls up or not. If you aren't heavily invested in the old stuff...try the new.
You need to leave a good margin around your work, a couple of inches all around, and anchor it down with some small kiln furniture at the corners and mid way along the edges too dependent upon how large your surface is (bits scrap glass works too...just be sure it's a good 1/2" away from your piece, or it will get pulled into the work as the paper shrinks). For larger work, it's just going to tear underneath no matter what. At least I haven't figured out a way around it. You can sprinkle the surface of the paper with some talc or dry primer to allow the glass to glide as the paper shrinks, but it may still tear.
The new thinfire doesn't shrink. I don't know if it curls up or not. If you aren't heavily invested in the old stuff...try the new.
i only used thinfire for a short while, when i was having problems with large bubbles forming under my glass. i had the same experience of it tearing because of the glass moving. i used two sheets of it a few times, which worked. i only left a margin of about an inch around the perimeter of my piece, and had little pieces of triangular kiln furniture as weights.
eventually i quit using thinfire altogether -- i figured out that i had a warped kiln shelf. when i bought a new shelf the bubble problem vanished. i still have about 75 sheets of the thinfire ... live and learn.
eventually i quit using thinfire altogether -- i figured out that i had a warped kiln shelf. when i bought a new shelf the bubble problem vanished. i still have about 75 sheets of the thinfire ... live and learn.
-
paulajane
I have been using the new thinfire since last summer. I have never had a problem I use it with small pieces as well as larger ones that are 10" x 8"
pictures. I cut the edges at an angle and anchor them with glass. The paper has never split or curled on me. I have a Skutt with top and side elements.
paulajane
pictures. I cut the edges at an angle and anchor them with glass. The paper has never split or curled on me. I have a Skutt with top and side elements.
paulajane
-
Catharine Newell
- Posts: 83
- Joined: Thu Mar 13, 2003 12:33 am
- Location: Portland, OR
-
Tony Serviente
- Posts: 328
- Joined: Thu May 29, 2003 11:48 am
- Location: Ithaca,NY
- Contact:
The new thin fire does not curl up or shrink. While it does not tear, it will wrinkle in the center of bigger pieces, a foot square and up or so. It is dense enough to cause bubble problems and it will also plug up a vaccuum filter about five times as fast as the old stuff. In spite of all that, I prefer it to the old.
-
Catharine Newell
- Posts: 83
- Joined: Thu Mar 13, 2003 12:33 am
- Location: Portland, OR
Tony,Tony Serviente wrote:The new thin fire does not curl up or shrink. While it does not tear, it will wrinkle in the center of bigger pieces, a foot square and up or so. It is dense enough to cause bubble problems and it will also plug up a vaccuum filter about five times as fast as the old stuff. In spite of all that, I prefer it to the old.
I wonder why you're having a problem with wrinkling??? I consistently fire panels 35x17 and have not had any experience with wrinkles...
Catharine
-
Tony Serviente
- Posts: 328
- Joined: Thu May 29, 2003 11:48 am
- Location: Ithaca,NY
- Contact:
-
Catharine Newell
- Posts: 83
- Joined: Thu Mar 13, 2003 12:33 am
- Location: Portland, OR
-
Tony Serviente
- Posts: 328
- Joined: Thu May 29, 2003 11:48 am
- Location: Ithaca,NY